Authors of this database present a data repository of Judd-Ofelt parameters for various kinds of host matrices, concentrations of RE ions, methods of preparations, etc. published by other authors in peer-reviewed scientific articles only. This approach ensures a diverse and rich data collection in a standardized format. The authors declare that presented data from trustable peer-review articles were not further checked and thus the authors of this database do not guarantee their factual correctness. If you find an incorrect record or irrelevant information, please get in touch with the authors and the record will be manually checked.
Reference:
- J. Hrabovsky, P. Varak, R. Krystufek, LOMS: interactive online software for Classical and Combinatorial Judd-Ofelt analysis with integrated database of Judd-Ofelt parameters, submitted to Scientific data, August 2024
Database Extension: Input form
- If you are interested in collaborating and expanding this database, please use the Submission form or send email to info@loms.cz
- If you have used the JO LOMS module for the calculation (JO analysis, Combinatorial JO analysis, transition analysis), it is also possible to attach input and output .csv files. In this case, please send the published results (PDF or link to peer-reviewed article) and .csv files as attachments to email: info@loms.cz
- JO paramaters database is also accessible via online Googlesheet (reading only, possible to download)
Notes:
- Units: Judd-Ofelt parameters (Ω2, Ω4,Ω6) are in 10-20 cm2 units
- Values in parentheses were not varied during the fitting procedure.
Abbreviations:
- Material type: Single crystal (SC), Polycrystal (PC), Polymer (Pol.), Glass (Glass), aquo, melt, vapor, solution
- Preparation method: Volumetric sample (bulk), Czochralski (Czoch.)
- Optical properties: Isotropic (Iso – default unless otherwise stated), Uniaxial (Uniax), Biaxial (Biax)
- JO analysis/Combinatorial JO analysis: combinatorial
RE ion | Host matrix | State | Comm. | Ω2 | Ω4 | Ω6 | Reference | LOMS files |
---|---|---|---|---|---|---|---|---|
Er | Te02-ZnO-BaO, TZB | Glass | 0.2mol.% Er203, Combinatorial JO analysis | 7.66 | 1.51 | 2.21 | Hrabovsky (2024) | LOMS |
Ho | YAG, Y3Al5O12 | SC | bulk SC | 0.101 | 2.086 | 1.724 | Walsh (2006) | LOMS |
Dy | YVO4 | SC | 1% Y for Dy | 6.59 | 3.71 | 1.74 | Cavalli (2002) | LOMS |
Dy | alpha-KGd(WO4)2 | SC | Czoch., 0.001-0.03mol.%RE | 9.878-15.347 | 3.053-14.631 | 2.006-19.966 | Kaminskii (2002) | LOMS |
Ho | YLF, LiYF4 | SC | Uniax., 0.5 % RE (1.38E22 cm-3) | 1.03 | 2.32 | 1.93 | Walsh (1998) | LOMS |
Nd | Y2O3 | SC | 3.1728 | 3.0819 | 1.9825 | Walsh (2002) | LOMS | |
Pm | PbO-P2O5-In2O3 | Glass | 0.5wt.% Pm2O3 | 3.8 | 2.4 | 2.6 | Shinn | LOMS |
Pr | RbPb2Cl5 | SC | Biax. | 10.63 | 9.22 | 3.72 | Merkle (2017) | LOMS |
Sm | Sr2SiO4 | PC | 0-0.07 mol.% Sm2O3 | 0.52 | 0.284 | 0.398 | Manjunath (2018) | LOMS |
Sm | TeO2-BiCl3 | Glass | 0.6mol.% Sm2O3 | 0.48 | 2.04 | 1.83 | Budchicha | LOMS |
Tb | LiTbF4 | SC | Uniax. | 1.5 | 2.23 | 2.06 | Vasyliev (2013) | LOMS |
Er | Ge-Ga-Sb-S | Glass | bulk, 0.5-5at.% | 3.40-5.8 | 1.80-2.46 | 1.85-1.96 | Strizik (2014) | LOMS |
Tm | GeO2-BaO/CaO-Na2O/Li2O | Glass | 2-4 mol.%. Tm2O3 | 6.14 | 1.54 | 0.87 | Walsh (2006) | LOMS |
Tm | S-FAP, Sr5(PO4)3F | SC | 3.1x1019 cm-3 | 7.633 | 10.48 | 3.281 | Bonner (2002) | LOMS |
Er | B2O3-K2O | Glass | bulk, 0.3 mol.% Er2O3 | 3.33-7.31 | 1.06-2.0 | 0.45-1.54 | Tanabe (1992) | |
Dy | B2O3-CaF2-CaO-BaO-Al2O3 | Glass | Bulk, 1 mol.% DyF3 | 5.98 | 2.33 | 2.33 | Kumar (2010) | |
Dy | H3BO3-BaF2 | Glass | Bulk, 1mol.% Dy2O3 | 2.91 | 1.09 | 0.98 | Dwivedi (2009) | |
Dy | YSGG, Y3Sc2ga3O12 | SC | Czoch, 0.5at.% Dy | 7.05 | 1.22 | 1.91 | Jamalaiah (2009) | |
Dy | PbO-B2O3-Al2O3-WO3 | Glass | 1 wt.% Dy | 4.9 | 0.94 | 2.07 | Pisarska (2009) | |
Dy | Li2CO3-H3BO3 | Glass | Bulk, 1mol.%Dy2O3 | 9.85-13.28 | 2.19-4.39 | 2.47-4.46 | Babu (2000) | |
Pr | Ge-Ga-S | Glass | Bulk | 12.8 | 4.3 | 7.7 | Wei (1995) | |
Pr | ZBLAN, ZrF4-BaF2-LaF3-AlF3-NaF | Glass | Bulk | 1.43 | 4.22 | 4.87 | Ohishi (1991) | |
Pr | ZBLA | Glass | Bulk | 0.24 | 4.5 | 5.4 | Eyal (1985) | |
Nd | B2O3-PbO | Glass | Bulk, 3mol.%Nd2O3 | 3.52-3.96 | 2.98-3.77 | 4.88-5.48 | Saisudha (1996) | |
Sm | B2O3-PbO | Glass | Bulk, 3mol.%Sm2O3 | 1.68-2.96 | 5-5.73 | 3.25-3.47 | Saisudha (1996) | |
Dy | B2O3-PbO | Glass | Bulk, 3mol.%Dy2O3 | 3.5-4.07 | 0.62-1.32 | 1.57-1.88 | Saisudha (1996) | |
Pr | ZBLAN, ZrF4-BaF2-LaF3-AlF3-NaF | Glass | Bulk, 3mol.% PrF3 | 0.84 | 4.79 | 9.13 | Wetenkamp (1992) | |
Tm | ZBLA, ZrF4-BaF2-LaF3-AlF3 | Glass | Bulk | 2.8 | 1.9 | 1 | Wetenkamp (1992) | |
Dy | ZBLALI, ZrF4-BaF2-LaF3-LiF | Glass | Bulk | 2.7 | 1.8 | 2 | Wetenkamp (1992) | |
Dy | ZBLAN, ZrF4-BaF2-LaF3-AlF3-NaF | Glass | Bulk, 3mol.% DyF3 | 1.86 | 1.42 | 2.37 | Wetenkamp (1992) | |
Nd | ZBLAN, ZrF4-BaF2-LaF3-AlF3-NaF | Glass | Bulk, 4mol.% NdF3 | 2.1 | 3.71 | 4.62 | Wetenkamp (1992) | |
Tm | ZBLAN, ZrF4-BaF2-LaF3-AlF3-NaF | Glass | Bulk, 4mol.% TmF3 | 2.7 | 1.59 | 1.09 | Wetenkamp (1992) | |
Er | ZBLAN, ZrF4-BaF2-LaF3-AlF3-NaF | Glass | Bulk | 2.97 | 1.23 | 1.17 | Wetenkamp (1992) | |
Er | ZBLAN, ZrF4-BaF2-LaF3-AlF3-NaF | Glass | Bulk, 4mol.% ErF3 | 2.91 | 1.78 | 1 | Wetenkamp (1992) | |
Ho | ZBLAN, ZrF4-BaF2-LaF3-AlF3-NaF | Glass | Bulk, 4mol.% HoF3 | 2.3 | 2.3 | 1.71 | Wetenkamp (1992) | |
Pr | ZBLA, ZrF4-BaF2-LaF3-AlF3 | Glass | Bulk, PrF3 | 0.06 | 5.05 | 6.92 | Adam (1985) | |
Nd | ZBLA, ZrF4-BaF2-LaF3-AlF3 | Glass | Bulk, NdF3 | 1.1 | 3.8 | 5.53 | Reisfeld (1986) | |
Nd | ZBN, ZrF4-BaF2-NaF | Glass | Bulk, 2 mol.%NdF3 | 1.95 | 3.65 | 4.17 | Lucas (1978) | |
Nd | ZBL, ZrF4-BaF2-LaF3 | Glass | Bulk, 1.7 mol.%NdF3 | 1.93 | 3.8 | 4.35 | Lucas (1978) | |
Nd | PBLA, PbF2-ZnF2-GaF3-AlF3-YF3-LaF3 | Glass | Bulk, 2 mol.%NdF3 | 1.01 | 3.73 | 6.19 | Reisfeld (1986) | |
Nd | ZnO-TeO2 | Glass | Bulk | 4.66 | 5.08 | 6.08 | Reisfeld (1986) | |
Ho | GLS, Ga2S3-La2S3 | Glass | Bulk | 2.31 | 2.81 | 1.08 | Reisfeld (1985) | |
Ho | ZBLA, ZrF4-BaF2-LaF3-AlF3 | Glass | Bulk | 2.43 | 1.67 | 1.84 | Reisfeld (1985) | |
Nd | GLS, Ga2S3-La2S3 | Glass | Bulk | 6.65 | 4.39 | 4.67 | Reisfeld (1985) | |
Pr | ZnO-TeO2 | Glass | Bulk | 2.59 | 7.26 | 5.45 | Hormadaly (1979) | |
Pr | BaO-TeO2 | Glass | Bulk | 4.95 | 6.46 | 5.44 | Hormadaly (1979) | |
Pr | Na2O-TeO2 | Glass | Bulk | 2.83 | 6.5 | 4.6 | Hormadaly (1979) | |
Pr | K2O-B2O3 | Glass | Bulk | 2.14 | 2.91 | 1.67 | Hormadaly (1979) | |
Pr | Na2O-B2O3 | Glass | Bulk | 0.77 | 4.13 | 3.07 | Hormadaly (1979) | |
Pr | Li2O-B2O3 | Glass | Bulk | 0.77 | 3.84 | 3.58 | Hormadaly (1979) | |
Dy | ZnO-TeO2 | Glass | Bulk | 4.28 | 1.32 | 2.53 | Hormadaly (1979) | |
Dy | BaO-TeO2 | Glass | Bulk | 3.2 | 1.35 | 2.47 | Hormadaly (1979) | |
Dy | Na2O-TeO2 | Glass | Bulk | 3.7 | 1.15 | 2.22 | Hormadaly (1979) | |
Dy | Na2O-P2O5 | Glass | Bulk | 1.46 | 1.16 | 1.97 | Hormadaly (1979) | |
Pr | Y2O3 | SC | Bulk | 17.21 | 19.8 | 4.88 | Krupke (1966) | |
Nd | Y2O3 | SC | Bulk | 8.55 | 5.25 | 2.89 | Krupke (1966) | |
Eu | Y2O3 | SC | Bulk | 6.31 | 0.66 | <0.48 | Krupke (1966) | |
Er | Y2O3 | SC | Bulk | 4.59 | 1.21 | 0.48 | Krupke (1966) | |
Tm | Y2O3 | SC | Bulk | 4.07 | 1.46 | 0.61 | Krupke (1966) | |
Pr | LaF3 | SC | Bulk | 0.12 | 1.77 | 4.78 | Krupke (1966) | |
Nd | LaF3 | SC | Bulk | 0.35 | 2.57 | 2.5 | Krupke (1966) | |
Pr | YAlO3 | SC | Bulk | 2 | 6 | 7 | Reisfeld (1985) | |
Nd | YAlO3 | SC | Bulk | 1.24 | 4.68 | 5.85 | Weber (1973) | |
Eu | YAlO3 | SC | Bulk | 2.66 | 6.32 | 0.8 | Weber (1973) | |
Tb | YAlO3 | SC | Bulk | 3.25 | 7.13 | 2 | Weber (1973) | |
Ho | YAlO3 | SC | Bulk | 1.82 | 2.38 | 1.53 | Weber (1973) | |
Er | YAlO3 | SC | Bulk | 1.06 | 2.63 | 0.78 | Weber (1973) | |
Tm | YAlO3 | SC | Bulk | 0.67 | 2.3 | 0.74 | Weber (1973) | |
Pr | YAG, Y3Al5O12 | SC | Bulk | 0.2 | 2.7 | 5 | Reisfeld (1985) | |
Er | GLS, Ga2S3-La2S3 | Glass | Bulk | 0.78 | 1.35 | 1.06 | Reisfeld (1985) | |
Eu | LaF3 | SC | Bulk | 1.19 | 1.16 | 0.39 | Reisfeld (1985) | |
Er | LaF3 | SC | Bulk | 1.07 | 0.28 | 0.63 | Weber (1967) | |
Ho | LaF3 | SC | Bulk | 1.16 | 1.38 | 0.88 | Weber (1972) | |
Er | ZBLA, ZrF4-BaF2-LaF3-AlF3 | Glass | Bulk | 2.54 | 1.39 | 0.97 | Shinn (1983) | |
Dy | LaF3 | SC | Bulk | 1.1 | 1.4 | 0.9 | Xu (1984) | |
Ho | ZBLA, ZrF4-BaF2-LaF3-AlF3 | Glass | Bulk | 2.28 | 2.08 | 1.73 | Tanimura (1984) | |
Er | ZBLA, ZrF4-BaF2-LaF3-AlF3 | Glass | Bulk | 3.26 | 1.85 | 1.14 | Reisfeld (1985) | |
Er | YSCZ, Yttria stabilized cubic zirconia crystal | SC | Bulk | 2.92 | 0.78 | 0.57 | Greenberg (1982) | |
Nd | ALS, Al2S3-La2S3 | Glass | Bulk | 9.45 | 4.84 | 6.54 | Reisfeld (1985) | |
Ho | ALS, Al2S3-La2S3 | Glass | Bulk | 8.09 | 3.85 | 1.4 | Reisfeld (1985) | |
Er | ALS, Al2S3-La2S3 | Glass | Bulk | 3.74 | 4.33 | 0.9 | Reisfeld (1985) | |
Ho | ZnO-TeO2 | Glass | Bulk | 6.92 | 2.81 | 1.42 | Reisfeld (1985) | |
Dy | ZBLA, ZrF4-BaF2-LaF3-AlF3 | Glass | Bulk | 3.22 | 1.35 | 2.38 | Adam (1988) | |
Tm | Silica, SiO2 | Glass | Bulk | 6.23 | 1.91 | 1.36 | Walsh (2004) | |
Tm | ZBLAN, ZrF4-BaF2-LaF3-AlF3-NaF | Glass | Bulk | 1.96 | 1.36 | 1.16 | Walsh (2004) | |
Er | ZBLANI, ZrF4-BaF2-LaF3-AlF3-NaF-InF3 | Glass | Bulk | 2.68-2.98 | 1.09-1.4 | 0.99-1.04 | Ivanova (2009) | |
Ho | PbO-Bi2O3-Ga2O3 | Glass | Bulk | 6.81 | 2.31 | 0.67 | Zhou (2009) | |
Ho | ZBLAN, ZrF4-BaF2-LaF3-AlF3-NaF | Glass | Bulk | 2.46 | 2.02 | 1.71 | Piatkowski (2008) | |
Ho | ZnO-TeO2 | Glass, 1mol.%Ho2O3 | Bulk | 5.28 | 3.42 | 1.2 | Boyer (2003) | |
Ho | PbO-ZnO-B2O3 | Glass, 1mol.%Ho2O3 | Bulk | 4.38 | 1.8 | 1.66 | Hussain (2006) | |
Ho | PbO-Al2O3-B2O3 | Glass | Bulk | 5.83 | 17.15 | 26.5 | Reddy (2000) | |
Sm | Na2O-SiO2 | Glass | Bulk, 0.3mol.%RE | 2.23-2.47 | 2.14-2.45 | 1.0-1.26 | Takebe (1995) | |
Er | Na2O-SiO2 | Glass | Bulk, 0.3mol.%RE | 4.07-4.37 | 0.64-0.83 | 0.23-0.32 | Takebe (1995) | |
Tm | Na2O-SiO2 | Glass | Bulk, 0.3mol.%RE | 2.16-2.63 | 0.16-0.38 | 0.43-0.5 | Takebe (1995) | |
Sm | Li2O-SiO2 | Glass | Bulk, 0.3mol.%RE | 2.55 | 3.77 | 1.82 | Takebe (1995) | |
Sm | Na2O-SiO2 | Glass | Bulk, 0.3mol.%RE | 2.47 | 2.32 | 1.26 | Takebe (1995) | |
Sm | K2O-SiO2 | Glass | Bulk, 0.3mol.%RE | 2.35 | 1.69 | 0.82 | Takebe (1995) | |
Sm | CaO-SiO2 | Glass | Bulk, 0.3mol.%RE | 2.73 | 4.44 | 2.03 | Takebe (1995) | |
Sm | SrO-SiO2 | Glass | Bulk, 0.3mol.%RE | 2.41 | 3.71 | 1.89 | Takebe (1995) | |
Sm | BaO-SiO2 | Glass | Bulk, 0.3mol.%RE | 2.51 | 3.32 | 1.69 | Takebe (1995) | |
Sm | Li2O-CaO-SiO2 | Glass | Bulk, 0.3mol.%RE | 2.43 | 4.23 | 2.07 | Takebe (1995) | |
Sm | Na2O-CaO-SiO2 | Glass | Bulk, 0.3mol.%RE | 2.64 | 3.3 | 1.64 | Takebe (1995) | |
Sm | K2O-CaO-SiO2 | Glass | Bulk, 0.3mol.%RE | 2.89 | 2.56 | 1.31 | Takebe (1995) | |
Sm | Na2O-B2O3 | Glass | Bulk, 0.3mol.%RE | 2.63-3.22 | 3.43-4.39 | 2.05-2.59 | Takebe (1995) | |
Sm | Li2O-B2O3 | Glass | Bulk, 0.3mol.%RE | 2.97 | 4.24 | 2.52 | Takebe (1995) | |
Sm | Na2O-B2O3 | Glass | Bulk, 0.3mol.%RE | 3.18 | 3.55 | 2.23 | Takebe (1995) | |
Sm | K2O-B2O3 | Glass | Bulk, 0.3mol.%RE | 2.59 | 2.03 | 1.52 | Takebe (1995) | |
Sm | CaO-B2O3 | Glass | Bulk, 0.3mol.%RE | 2.87 | 4.29 | 2.42 | Takebe (1995) | |
Sm | SrO-B2O3 | Glass | Bulk, 0.3mol.%RE | 2.94 | 4.29 | 2.52 | Takebe (1995) | |
Sm | BaO-B2O3 | Glass | Bulk, 0.3mol.%RE | 2.94 | 3.98 | 2.41 | Takebe (1995) | |
Sm | Na2O-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 2.49-2.68 | 3.63-4.0 | 2.22-2.26 | Takebe (1995) | |
Sm | Li2O-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 2.71 | 3.37 | 2.11 | Takebe (1995) | |
Sm | Na2O-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 2.59 | 3.63 | 2.26 | Takebe (1995) | |
Sm | K2O-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 3.41 | 3.82 | 2.27 | Takebe (1995) | |
Sm | MgO--P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 3.48 | 2.9 | 1.78 | Takebe (1995) | |
Sm | CaO-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 3.13 | 3.09 | 1.81 | Takebe (1995) | |
Sm | SrO-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 3.34 | 3.29 | 2.01 | Takebe (1995) | |
Sm | BaO-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 3.08 | 3.21 | 2.02 | Takebe (1995) | |
Er | Li2O-SiO2 | Glass | Bulk, 0.3mol.%RE | 4.69 | 1.29 | 0.56 | Takebe (1995) | |
Er | Na2O-SiO2 | Glass | Bulk, 0.3mol.%RE | 4.37 | 0.83 | 0.27 | Takebe (1995) | |
Er | K2O-SiO2 | Glass | Bulk, 0.3mol.%RE | 5.02 | 0.71 | 0.24 | Takebe (1995) | |
Er | CaO-SiO2 | Glass | Bulk, 0.3mol.%RE | 5.91 | 1.53 | 0.77 | Takebe (1995) | |
Er | SrO-SiO2 | Glass | Bulk, 0.3mol.%RE | 5.22 | 1.25 | 0.61 | Takebe (1995) | |
Er | BaO-SiO2 | Glass | Bulk, 0.3mol.%RE | 3.42 | 0.83 | 0.27 | Takebe (1995) | |
Er | Li2O-CaO-SiO2 | Glass | Bulk, 0.3mol.%RE | 4.96 | 1.41 | 0.65 | Takebe (1995) | |
Er | Na2O-CaO-SiO2 | Glass | Bulk, 0.3mol.%RE | 5.22 | 1.02 | 0.48 | Takebe (1995) | |
Er | K2O-CaO-SiO2 | Glass | Bulk, 0.3mol.%RE | 5.63 | 0.99 | 0.34 | Takebe (1995) | |
Er | Na2O-B2O3 | Glass | Bulk, 0.3mol.%RE | 3.31-6.17 | 1.3-2.07 | 0.73-1.57 | Takebe (1995) | |
Er | Li2O-B2O3 | Glass | Bulk, 0.3mol.%RE | 5.81 | 1.84 | 1.18 | Takebe (1995) | |
Er | Na2O-B2O3 | Glass | Bulk, 0.3mol.%RE | 6.04 | 1.59 | 0.91 | Takebe (1995) | |
Er | K2O-B2O3 | Glass | Bulk, 0.3mol.%RE | 5.38 | 1.02 | 0.44 | Takebe (1995) | |
Er | CaO-B2O3 | Glass | Bulk, 0.3mol.%RE | 6.33 | 1.96 | 1.25 | Takebe (1995) | |
Er | SrO-B2O3 | Glass | Bulk, 0.3mol.%RE | 6.06 | 1.87 | 1.18 | Takebe (1995) | |
Er | BaO-B2O3 | Glass | Bulk, 0.3mol.%RE | 6.57 | 1.84 | 1.01 | Takebe (1995) | |
Er | Na2O-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 6.17-6.8 | 1.53-1.78 | 0.91-1.17 | Takebe (1995) | |
Er | Li2O-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 6.42 | 1.64 | 0.78 | Takebe (1995) | |
Er | Na2O-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 6.85 | 1.67 | 1.08 | Takebe (1995) | |
Er | K2O-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 6.94 | 1.84 | 1.1 | Takebe (1995) | |
Er | MgO--P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 6.69 | 1.02 | 0.63 | Takebe (1995) | |
Er | CaO-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 6.77 | 1.33 | 0.69 | Takebe (1995) | |
Er | SrO-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 6.63 | 1.53 | 0.7 | Takebe (1995) | |
Er | BaO-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 6.34 | 1.74 | 0.81 | Takebe (1995) | |
Tm | Li2O-SiO2 | Glass | Bulk, 0.3mol.%RE | 2.39 | 0.77 | 0.61 | Takebe (1995) | |
Tm | Na2O-SiO2 | Glass | Bulk, 0.3mol.%RE | 2.16 | 0.16 | 0.5 | Takebe (1995) | |
Tm | K2O-SiO2 | Glass | Bulk, 0.3mol.%RE | 2.54 | 0.07 | 0.45 | Takebe (1995) | |
Tm | CaO-SiO2 | Glass | Bulk, 0.3mol.%RE | 3.59 | 0.99 | 0.86 | Takebe (1995) | |
Tm | SrO-SiO2 | Glass | Bulk, 0.3mol.%RE | 3.17 | 0.69 | 0.66 | Takebe (1995) | |
Tm | BaO-SiO2 | Glass | Bulk, 0.3mol.%RE | 2.69 | 0.7 | 0.55 | Takebe (1995) | |
Tm | Li2O-CaO-SiO2 | Glass | Bulk, 0.3mol.%RE | 2.81 | 1.02 | 0.7 | Takebe (1995) | |
Tm | Na2O-CaO-SiO2 | Glass | Bulk, 0.3mol.%RE | 2.68 | 0.64 | 0.53 | Takebe (1995) | |
Tm | K2O-CaO-SiO2 | Glass | Bulk, 0.3mol.%RE | 3.33 | 0.53 | 0.52 | Takebe (1995) | |
Tm | Na2O-B2O3 | Glass | Bulk, 0.3mol.%RE | 2.41-4.01 | 0.72-2.44 | 0.87-1.53 | Takebe (1995) | |
Tm | Li2O-B2O3 | Glass | Bulk, 0.3mol.%RE | 3.87 | 1.77 | 1.28 | Takebe (1995) | |
Tm | Na2O-B2O3 | Glass | Bulk, 0.3mol.%RE | 3.37 | 0.99 | 0.96 | Takebe (1995) | |
Tm | K2O-B2O3 | Glass | Bulk, 0.3mol.%RE | 3.03 | 0.29 | 0.7 | Takebe (1995) | |
Tm | CaO-B2O3 | Glass | Bulk, 0.3mol.%RE | 3.83 | 1.82 | 1.31 | Takebe (1995) | |
Tm | SrO-B2O3 | Glass | Bulk, 0.3mol.%RE | 3.95 | 1.54 | 1.28 | Takebe (1995) | |
Tm | BaO-B2O3 | Glass | Bulk, 0.3mol.%RE | 4.28 | 1.61 | 1.23 | Takebe (1995) | |
Tm | Na2O-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 3.64-3.84 | 0.94-1.32 | 0.85-1.05 | Takebe (1995) | |
Tm | Li2O-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 3.69 | 1.23 | 0.93 | Takebe (1995) | |
Tm | Na2O-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 3.84 | 1.32 | 0.98 | Takebe (1995) | |
Tm | K2O-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 3.6 | 1.32 | 1.17 | Takebe (1995) | |
Tm | MgO--P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 3.85 | 0.69 | 0.72 | Takebe (1995) | |
Tm | CaO-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 3.96 | 0.93 | 0.74 | Takebe (1995) | |
Tm | SrO-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 3.6 | 0.79 | 0.82 | Takebe (1995) | |
Tm | BaO-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 3.27 | 0.98 | 0.81 | Takebe (1995) | |
Pr | Li2O-CaO-SiO2 | Glass | Bulk, 0.3mol.%RE | 2.69 | 6.01 | 4.7 | Takebe (1995) | |
Pr | Na2O-CaO-SiO2 | Glass | Bulk, 0.3mol.%RE | 3.91 | 5.72 | 3.82 | Takebe (1995) | |
Pr | K2O-CaO-SiO2 | Glass | Bulk, 0.3mol.%RE | 5.16 | 5.21 | 2.5 | Takebe (1995) | |
Pr | Na2O-SiO2 | Glass | Bulk, 0.3mol.%RE | 4.81 | 4.71 | 3.01 | Takebe (1995) | |
Pr | Li2O-B2O3 | Glass | Bulk, 0.3mol.%RE | 0.1 | 4.71 | 5.28 | Takebe (1995) | |
Pr | Na2O-B2O3 | Glass | Bulk, 0.3mol.%RE | 0.98 | 4.76 | 4.86 | Takebe (1995) | |
Pr | K2O-B2O3 | Glass | Bulk, 0.3mol.%RE | 2.33 | 4.65 | 3.84 | Takebe (1995) | |
Pr | CaO-B2O3 | Glass | Bulk, 0.3mol.%RE | -0.1 | 4.75 | 5.12 | Takebe (1995) | |
Pr | BaO-B2O3 | Glass | Bulk, 0.3mol.%RE | 0.5 | 4.98 | 5 | Takebe (1995) | |
Pr | Li2O-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 2.41 | 5.89 | 5.6 | Takebe (1995) | |
Pr | Na2O-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 2.06 | 6.41 | 5.61 | Takebe (1995) | |
Pr | MgO--P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 6.44 | 4.52 | 3.95 | Takebe (1995) | |
Pr | CaO-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 5.28 | 5.2 | 4.34 | Takebe (1995) | |
Pr | BaO-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 3.53 | 5.66 | 4.77 | Takebe (1995) | |
Nd | Li2O-CaO-SiO2 | Glass | Bulk, 0.3mol.%RE | 3.63 | 4.21 | 4.94 | Takebe (1995) | |
Nd | Na2O-CaO-SiO2 | Glass | Bulk, 0.3mol.%RE | 4.64 | 3.81 | 4.17 | Takebe (1995) | |
Nd | K2O-CaO-SiO2 | Glass | Bulk, 0.3mol.%RE | 5.23 | 3.1 | 3.14 | Takebe (1995) | |
Nd | Na2O-SiO2 | Glass | Bulk, 0.3mol.%RE | 4.83 | 3.07 | 3.37 | Takebe (1995) | |
Nd | Li2O-B2O3 | Glass | Bulk, 0.3mol.%RE | 4.2 | 3.89 | 4.74 | Takebe (1995) | |
Nd | Na2O-B2O3 | Glass | Bulk, 0.3mol.%RE | 4.91 | 3.28 | 4.51 | Takebe (1995) | |
Nd | K2O-B2O3 | Glass | Bulk, 0.3mol.%RE | 4.94 | 3.1 | 3.42 | Takebe (1995) | |
Nd | CaO-B2O3 | Glass | Bulk, 0.3mol.%RE | 4.36 | 3.74 | 4.64 | Takebe (1995) | |
Nd | BaO-B2O3 | Glass | Bulk, 0.3mol.%RE | 4.65 | 3.56 | 4.74 | Takebe (1995) | |
Nd | Li2O-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 3.71 | 4.7 | 5.15 | Takebe (1995) | |
Nd | Na2O-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 3.82 | 4.74 | 5.53 | Takebe (1995) | |
Nd | MgO--P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 5.72 | 3.69 | 4.31 | Takebe (1995) | |
Nd | CaO-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 5.27 | 3.77 | 4.34 | Takebe (1995) | |
Nd | BaO-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 4.37 | 4.05 | 4.82 | Takebe (1995) | |
Tb | Li2O-CaO-SiO2 | Glass | Bulk, 3mol.%RE | 0.75 | 2.11 | Takebe (1995) | ||
Tb | Na2O-CaO-SiO2 | Glass | Bulk, 3mol.%RE | 0.68 | 1.39 | Takebe (1995) | ||
Tb | K2O-CaO-SiO2 | Glass | Bulk, 3mol.%RE | 0.61 | 1.05 | Takebe (1995) | ||
Tb | Na2O-SiO2 | Glass | Bulk, 3mol.%RE | 0.48 | 0.78 | Takebe (1995) | ||
Tb | Li2O-B2O3 | Glass | Bulk, 3mol.%RE | 5.56 | 1.33 | 3.22 | Takebe (1995) | |
Tb | Na2O-B2O3 | Glass | Bulk, 3mol.%RE | 8.82 | 0.85 | 2.8 | Takebe (1995) | |
Tb | K2O-B2O3 | Glass | Bulk, 3mol.%RE | 0.73 | 1.76 | Takebe (1995) | ||
Tb | CaO-B2O3 | Glass | Bulk, 3mol.%RE | 6.95 | 1.28 | 2.91 | Takebe (1995) | |
Tb | BaO-B2O3 | Glass | Bulk, 3mol.%RE | 6.72 | 0.95 | 2.81 | Takebe (1995) | |
Tb | Li2O-P2O5-Al2O3 | Glass | Bulk, 3mol.%RE | 6.44 | 1.05 | 2.21 | Takebe (1995) | |
Tb | Na2O-P2O5-Al2O3 | Glass | Bulk, 3mol.%RE | 6.8 | 1.11 | 2.27 | Takebe (1995) | |
Tb | MgO--P2O5-Al2O3 | Glass | Bulk, 3mol.%RE | 8.41 | 0.86 | 1.31 | Takebe (1995) | |
Tb | CaO-P2O5-Al2O3 | Glass | Bulk, 3mol.%RE | 7.51 | 0.79 | 1.6 | Takebe (1995) | |
Tb | BaO-P2O5-Al2O3 | Glass | Bulk, 3mol.%RE | 7.26 | 0.9 | 2.03 | Takebe (1995) | |
Dy | Li2O-CaO-SiO2 | Glass | Bulk, 0.3mol.%RE | 4.03 | 2.47 | 1.07 | Takebe (1995) | |
Dy | Na2O-CaO-SiO2 | Glass | Bulk, 0.3mol.%RE | 4.44 | 1.51 | 0.71 | Takebe (1995) | |
Dy | K2O-CaO-SiO2 | Glass | Bulk, 0.3mol.%RE | 5.19 | 1.35 | 0.61 | Takebe (1995) | |
Dy | Na2O-SiO2 | Glass | Bulk, 0.3mol.%RE | 4.24 | 1.09 | 0.47 | Takebe (1995) | |
Dy | Li2O-B2O3 | Glass | Bulk, 0.3mol.%RE | 4.56 | 3.14 | 1.78 | Takebe (1995) | |
Dy | Na2O-B2O3 | Glass | Bulk, 0.3mol.%RE | 5.3 | 2.52 | 1.53 | Takebe (1995) | |
Dy | K2O-B2O3 | Glass | Bulk, 0.3mol.%RE | 5.29 | 1.4 | 0.78 | Takebe (1995) | |
Dy | CaO-B2O3 | Glass | Bulk, 0.3mol.%RE | 4.9 | 3.29 | 1.74 | Takebe (1995) | |
Dy | BaO-B2O3 | Glass | Bulk, 0.3mol.%RE | 4.96 | 2.99 | 1.61 | Takebe (1995) | |
Dy | Li2O-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 4.92 | 2.28 | 1.54 | Takebe (1995) | |
Dy | Na2O-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 5.31 | 2.62 | 1.62 | Takebe (1995) | |
Dy | MgO--P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 6.58 | 1.57 | 1.09 | Takebe (1995) | |
Dy | CaO-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 6.23 | 1.56 | 1.21 | Takebe (1995) | |
Dy | BaO-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 5.36 | 2.39 | 1.33 | Takebe (1995) | |
Ho | Li2O-CaO-SiO2 | Glass | Bulk, 0.3mol.%RE | 5.87 | 1.94 | 1.22 | Takebe (1995) | |
Ho | Na2O-CaO-SiO2 | Glass | Bulk, 0.3mol.%RE | 6.42 | 1.46 | 0.65 | Takebe (1995) | |
Ho | K2O-CaO-SiO2 | Glass | Bulk, 0.3mol.%RE | 6.81 | 1.39 | 0.43 | Takebe (1995) | |
Ho | Na2O-SiO2 | Glass | Bulk, 0.3mol.%RE | 6.04 | 0.9 | 0.24 | Takebe (1995) | |
Ho | Li2O-B2O3 | Glass | Bulk, 0.3mol.%RE | 5.9 | 1.82 | 2.02 | Takebe (1995) | |
Ho | Na2O-B2O3 | Glass | Bulk, 0.3mol.%RE | 6.85 | 1.64 | 1.61 | Takebe (1995) | |
Ho | K2O-B2O3 | Glass | Bulk, 0.3mol.%RE | 6.62 | 0.99 | 0.63 | Takebe (1995) | |
Ho | CaO-B2O3 | Glass | Bulk, 0.3mol.%RE | 5.99 | 2.01 | 1.96 | Takebe (1995) | |
Ho | BaO-B2O3 | Glass | Bulk, 0.3mol.%RE | 6.44 | 1.66 | 1.84 | Takebe (1995) | |
Ho | Li2O-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 6.19 | 1.8 | 1.5 | Takebe (1995) | |
Ho | Na2O-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 6.7 | 1.98 | 1.73 | Takebe (1995) | |
Ho | MgO--P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 8.21 | 1.38 | 1.14 | Takebe (1995) | |
Ho | CaO-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 8.13 | 1.48 | 1.21 | Takebe (1995) | |
Ho | BaO-P2O5-Al2O3 | Glass | Bulk, 0.3mol.%RE | 7.11 | 1.75 | 1.47 | Takebe (1995) | |
Er | ZBLAN, ZrF4-BaF2-LaF3-AlF3-NaF | Glass | Bulk, 1mol.%RE | 2.97 | 1.59 | 1.04 | Wang (2009) | |
Er | ZBLAN, ZrF4-BaF2-LaF3-AlF3-NaF | Glass | Bulk | 2.2 | 1.4 | 0.91 | Wang (2009) | |
Er | ZBLAN, ZrF4-BaF2-LaF3-AlF3-NaF | Glass | Bulk | 2.97 | 1.23 | 1.17 | Yanagita (1991) | |
Nd | KTG, K2O-Ta2O5-Ga2O3 | Glass | Bulk | 11.4 | 5.04 | 5.57 | Takebe (1997) | |
Nd | PbO-Bi2O3-Ga2O3 | Glass | Bulk | 3.72 | 4.48 | 4.33 | Takebe (1997) | |
Nd | ZBLAN | Glass | Bulk | 2.37 | 3.77 | 4.85 | Takebe (1997) | |
Nd | Ge-Ga-S | Glass | Bulk | 10.6 | 9.56 | 6.04 | Takebe (1997) | |
Er | Na2O-GeO2-SiO2 | Glass | Bulk, 0.1 mol.% RE2O3 | 4.43 | 0.64 | 0.38 | Varak (2022) | |
Er | Na2O-ZnO-SiO2 | Glass | Bulk, 0.1 mol.% RE2O3 | 5.23 | 0.72 | 0.53 | Varak (2022) | |
Er | Na2O-Al2O3-SiO2 | Glass | Bulk, 0.1 mol.% RE2O3 | 4.81 | 0.8 | 0.42 | Varak (2022) | |
Ho | Na2O-GeO2-SiO2 | Glass | Bulk, 0.1 mol.% RE2O3 | 4.23 | 0.74 | 0.7 | Varak (2022) | |
Ho | Na2O-ZnO-SiO2 | Glass | Bulk, 0.1 mol.% RE2O3 | 5.15 | 1.03 | 0.93 | Varak (2022) | |
Ho | Na2O-Al2O3-SiO2 | Glass | Bulk, 0.1 mol.% RE2O3 | 4.81 | 0.83 | 0.74 | Varak (2022) | |
Pr | TeO2-PbF2-AlF3 | Glass | Bulk, 2.5 mol. % REF3 | 0.62 | 1.39 | 13.19 | Lalla (2020) | |
Nd | TeO2-PbF2-AlF3 | Glass | Bulk, 2.5 mol. % REF3 | 4.51 | 6.34 | 6.16 | Lalla (2020) | |
Sm | TeO2-PbF2-AlF3 | Glass | Bulk, 2.5 mol. % REF3 | 1.11 | 3.92 | 3.29 | Lalla (2020) | |
Dy | TeO2-PbF2-AlF3 | Glass | Bulk, 2.5 mol. % REF3 | 8.53 | 1.58 | 3.51 | Lalla (2020) | |
Ho | TeO2-PbF2-AlF3 | Glass | Bulk, 2.5 mol. % REF3 | 3.75 | 2.38 | 1.6 | Lalla (2020) | |
Er | TeO2-PbF2-AlF3 | Glass | Bulk, 2.5 mol. % REF3 | 5.52 | 2.07 | 1 | Lalla (2020) | |
Tm | TeO2-PbF2-AlF3 | Glass | Bulk, 2.5 mol. % REF3 | 5.01 | 2.64 | 1.37 | Lalla (2020) | |
Ho | TeO2-ZnO-BaF2 | Glass | Bulk, 0.5 mol. % Ho2O3 | 3.562 | 4.666 | 2.26 | Kumi-Barimah (2022) | |
Ho | SiO2-GeO2-CaO-K2O3-Na2O-Nb2O5 | Glass | Bulk, 0.5 mol. % Ho2O3 | 4.4 | 2.78 | 1.21 | Chen (2017) | |
Sm | Y2O3 | PC | Bulk, 3 at. % Sm | 1.37 | 1.61 | 0.87 | Hu (2023) | |
Dy | YAG, Y3Al5O12 | SC | 1.98 at. % Dy | 2.34 | 3.04 | 3.83 | Li (2022) | |
Dy | YAG, Y3Al5O12 | SC | 2 at. % Dy | 0.498 | 2.155 | 2.848 | Yang (2023) | |
Dy | YAG, Y3Al5O12 | SC | (Dy0.03Y0.97)3Al5O12 | 1.49 | 0.94 | 3.2 | Pan (2018) | |
Dy | LiYF4 | SC | 2.01 | 1.34 | 2.39 | Brik (2004) | ||
Dy | Lu2SiO5 | SC | 1 at. % Dy | 4.31 | 1.28 | 3.49 | Dominiak-Dzik (2009) | |
Dy | TeO2-BiCl3 | Glass | 0.6mol.% Nd2O3 | 4.91 | 0.63 | 2.29 | Budchicha | |
Dy | Bi4Si3O12 | SC | 0.2% Bi for Dy | 1.38 | 0.18 | 0.35 | Zhang (2014) | |
Dy | Y3Sc2Ga3O12 | SC | 0.5 at. % Dy | 0.13 | 0.73 | 1.06 | Sardar (2004) | |
Dy | Gd3Ga5O12 | SC | 0.17 | 2.66 | 2.57 | Wang (2010) | ||
Dy | YAG, Y3Al5O12 | PC | 5 at. % Dy | 0.2 | 1.11 | 1.46 | Lupei (2011) | |
Nd | YAG, Y3Al5O12 | SC | 0.2 wt% Nd | 0.5022 | 3.3506 | 5.1653 | Guo (2013) | |
Nd | YAG, Y3Al5O12 | PC | 1% Nd | 0.64 | 2.58 | 4.06 | Strek (2007) | |
Nd | SiO2–Na2O–PbO–ZnO | Glass | 3.66 | 5.53 | 2.73 | Serqueira (2006) | ||
Nd | Calcium Aluminate | Glass | 0.5 mol. % Nd2O3 | 4.87 | 5.5 | 3.42 | Uhlmann (1994) | |
Nd | CaZn2Y2Ge3O12 | SC | 2 at. % Nd | 0.98 | 3.2 | 3.63 | Sardar (1994) | |
Nd | YAG, Y3Al5O12 | SC | 0.76 at. % Nd | 0.2 | 2.7 | 5 | Krupke (1971) | |
Nd | CaO-Al2O3-MgO-SiO2 | Glass | 2.5 wt.% Nd2O3 | 3.34 | 4.42 | 2.02 | Pecoraro (2000) | |
Nd | YAG, Y3Al5O12 | SC | 1 at. % Nd | 0.202 | 2.615 | 5.305 | Li (2012) | |
Nd | YAG, Y3Al5O12 | PC | 0.9 at. % Nd | 0.23 | 3.3 | 5 | Kumar (2004) | |
Nd | YAG, Y3Al5O12 | PC | 1 at. % Nd | 0.224 | 2.567 | 3.712 | Sardar (2006) | |
Nd | Y2O3 | PC | 1 at. % Nd | 4.364 | 3.609 | 2.919 | Hou (2011) | |
Nd | YAG, Y3Al5O12 | PC | 5 at. % Nd | 0.38 | 4.06 | 5.36 | Sato (2003) | |
Nd | YScAG, Y3Sc2Al3O12 | PC | 5 at. % Nd | 0.1 | 3.22 | 3.81 | Sato (2003) | |
Nd | TeO2-BiCl3 | Glass | 0.6mol.% Nd2O3 | 3.34 | 3.86 | 3.54 | Budchicha | |
Er | TeO2-BiCl3 | Glass | 0.6mol.% Er2O3 | 3.38 | 0.72 | 1.55 | Budchicha | |
Er | Bi2O3-B2O3-Na2O | Glass | bulk, 1mol.%, Er2O3 | 3.86 | 1.52 | 1.17 | Yang (2003) | |
Tb | TbCaF | SC | Uniax. | 1.14 | 1.52 | 1.82 | Vasyliev (2013) | |
Tm | FAP, Ca3(PO4)3F | SC | 9x1019 cm-3 | 7.593 | 2.406 | 1.141 | Bonner (2002) | |
Tm | B-FAP, Ba5(PO4)3F | SC | 3.5x1019 cm-3 | 29.18 | 4.185 | 2.018 | Bonner (2002) | |
Ho | LuAG Lu3Al5O12 | SC | bulk SC | 0.125 | 1.987 | 1.656 | Walsh (2006) | |
Nd | TeO2-BiCl3 | Glass | 0.6mol.% RE2O3 | 3.34 | 3.86 | 3.54 | Bouchicha (2023) | |
Sm | TeO2-BiCl3 | Glass | 0.6mol.% RE2O3 | 0.48 | 2.04 | 1.83 | Bouchicha (2023) | |
Dy | TeO2-BiCl3 | Glass | 0.6mol.% RE2O3 | 4.91 | 0.63 | 2.29 | Bouchicha (2023) | |
Er | TeO2-BiCl3 | Glass | 0.6mol.% RE2O3 | 3.38 | 0.72 | 1.55 | Bouchicha (2023) | |
Pr | TLF, TeO2-LiF | Glass | 10 mol.%REO | 1.8-3.11 | 3.69-3.92 | 7.89-10.70 | Kumar (2001) | |
Nd | TLF, TeO2-LiF | Glass | 10 mol.%REO | 5.61 | 4.17 | 5.44 | Kumar (2001) | |
Er | TLF, TeO2-LiF | Glass | 10 mol.%REO | 7.14 | 0.74 | 2.18 | Kumar (2001) | |
Nd | TeO2-B2O3-ZnF2-BaO | Glass | 0-1.5 mol.% RE2O3 | 2.89 | 1.35 | 1.59 | Yuliantini (2021) | |
Nd | TeO2-PbF2-AlF3 | Glass | 0.01-2.5 mol.% NdF3 | 4.21-4.51 | 5.97-6.34 | 5.45-6.16 | Lalla (2016) | |
Nd | P2O5-ZnO | Glass | 0-2 mol.%- Nd2O3 | 3.76-6.13 | 1.16-5.67 | 3.23-6.83 | Mahraz (2019) | |
Nd | TeO2-WO3 | Glass | 0-4 mol.%- Nd2O3 | 4.6 | 3.3 | 3.5 | Costa (2016) | |
Sm | Li2CO3-H3BO3-ZnF2 | Glass | 1 mol.% Sm2O3 | 1.73 | 9.45 | 8.93 | Thomas (2013) | |
Sm | PbO-H3BO3-TiO2-AlF3 | Glass | 0.1-2 mol.%- Sm2O3 | 0.27 | 2.52 | 2.47 | Jamalaiah (2009) | |
Er | B2O3-Na2O | Glass | bulk, 0.3 mol.%, Er2O3 | 3.21-6.11 | 1.13-1.98 | 0.6-1.39 | Tanabe (1992) | |
Tm | GeO2-PbO | Glass | 2.81 | 0.29 | 0.86 | Wechtler (1998) | ||
Tm | GeO2-PbO-Nb2O5 | Glass | 5.55 | 2.03 | 1.26 | Balda (2005) | ||
Tm | GeO2-BaO-K2O | Glass | 3.53 | 1.38 | 0.71 | Reisfeld (1975) | ||
Tm | GeO2-BaO-K2O | Glass | 4 | 1.6 | 0.8 | Reisfeld (1978) | ||
Ho | YAG, Y3Al5O12 | SC | bulk Czoch., SC | 0.04 | 2.67 | 1.89 | Malinowski (2000) | |
Tm | YLF, LiYF4 | SC | Uniax., 0.5 % RE (1.38E22 cm-3) | 1.67 | 1.93 | 1.1 | Walsh (1998) | |
Tm | YLF, LiYF4 | SC | Uniax. | 2.52 | 1.04 | 0.68 | Dulick (1991) | |
Tm | YLF, LiYF4 | SC | Uniax. | 3.54 | 0.29 | 1.4 | Walsh (1998) | |
Ho | LuAG Lu3Al5O12 | SC | bulk, SC | 0.172 | 2.08 | 1.92 | Patel (1998) | |
Ho | YLF, LiYF4 | SC | Uniax. | 0.96 | 2.05 | 1.43 | Walsh (1998) | |
Ho | YLF, LiYF4 | SC | Uniax. | 1.16 | 1.62 | 1.6 | Walsh (1998) | |
Yb | (aquo) | (aquo) | 0.93 | 1.76 | 1.89 | Carnal (1965) | ||
Yb | (aquo) | (aquo) | 0.8 | (1.6) | (1.6) | Beltyukova (1977) | ||
Yb | EDTA | solution | (1:2) | 5.5 | (1.6) | (1.6) | Beltyukova (1977) | |
Yb | Antipyryne | solution | (1:5) | 6 | (1.6) | (1.6) | Beltyukova (1977) | |
Yb | EDTA | solution | (1:3) | 9.2 | (1.6) | (1.6) | Beltyukova (1977) | |
Yb | NTA | solution | (1:5) | 9.6 | (1.6) | (1.6) | Beltyukova (1977) | |
Yb | MAL | solution | (1:5) | 11.1 | (1.6) | (1.6) | Beltyukova (1977) | |
Yb | sulfosalicylic acid | solution | (1:2) | 11.9 | (1.6) | (1.6) | Beltyukova (1977) | |
Yb | citric acid | solution | (1:5) | 13.6 | (1.6) | (1.6) | Beltyukova (1977) | |
Yb | LiNO3-KNO3 | melt | 13.1 | 2.32 | 1.55 | Carnal (1965) | ||
Yb | maleic acid | solution | (1:5) | 13.1 | (1.6) | (1.6) | Beltyukova (1977) | |
Yb | nitriloacetic acid | solution | (1:2) | 15.6 | (1.6) | (1.6) | Beltyukova (1977) | |
Yb | trihydroxyglutatic acid | solution | (1:5) | 19.3 | (1.6) | (1.6) | Beltyukova (1977) | |
Yb | malic acid | solution | (1:5) | 20 | (1.6) | (1.6) | Beltyukova (1977) | |
Yb | tartaric acid | solution | (1:5) | 20 | (1.6) | (1.6) | Beltyukova (1977) | |
Yb | acetylacetone | solution | (1:10) | 26.7 | (1.6) | (1.6) | Beltyukova (1977) | |
Yb | benzoylacetone | solution | (1:10) | 28.9 | (1.6) | (1.6) | Beltyukova (1977) | |
Yb | thenoyltrifluoro-acetone | solution | (1:10) | 30.9 | (1.6) | (1.6) | Beltyukova (1977) | |
Yb | DBM | solution | (1:10) | 32.8 | (1.6) | (1.6) | Beltyukova (1977) | |
Yb | sulfosalicylic acid | solution | (1:40) | 36.9 | (1.6) | (1.6) | Beltyukova (1977) | |
Tm | LaF3 | crystal | 0.52 | 0.59 | 0.22 | Leavitt (1980) | ||
Tm | Tm(C2H5SO4)3·9H2O | crystal | 0.593 | 2.248 | 1.251 | Krupke (1965) | ||
Tm | (aquo) | (aquo) | 0.646 | 2.31 | 1.47 | Carnall (1983) | ||
Tm | YAG,Y3Al5O12 | crystal | 0.7 | 1.2 | 0.5 | Weber (1973) | ||
Tm | BZYT fluoride | Glass | 1.14 | 1.57 | 1.13 | Yeh (1988) | ||
Tm | AlPO4–AlF3–PbF2–CaF2–YbF3 | Glass | TmF3 | 1.3 | 1 | 1.5 | Ozen (1993) | |
Tm | AlPO4–AlF3–PbF2–CaF2 | Glass | TmF3 | 1.38 | 0.75 | 0.92 | Ozen (1995) | |
Tm | K7[TmW10O35] | 1.58 | 5.78 | 0.83 | Peacock (1973) | |||
Tm | PZG fluoride | Glass | 1.71 | 1.46 | 1.06 | Eyal (1987b) | ||
Tm | AlF3–CaF2–BaF2–YF3 | Glass | TmF3 | 1.75 | 1.33 | 1.27 | Tanabe (1993) | |
Tm | ZnF2–AlF3–BaF2–SrF2–YF3 | Glass | 1.83 | 1.7 | 1.12 | Tanabe (1996) | ||
Tm | BIGaZYTZr fluoride | glass | 1.mol% | 1.89 | 1.56 | 1.09 | Joubert (1995) | |
Tm | AlF3–ZrF4–MgF2–CaF2–SrF2–BaF2–NaF–NaCl | Glass | 1.92 | 1.68 | 1.13 | Peng (1995) | ||
Tm | ZBLA | Glass | 1.94 | 1.63 | 0.74 | Gorller-Walrand (1998) | ||
Tm | ZBLAK | Glass | 1.98 | 1.54 | 0.56 | Gorller-Walrand (1998) | ||
Tm | AlF3–CaF2–BaF2–YF3 | Glass | TmF3 | 1.98 | 1.32 | 1.07 | Hirao (1993) | |
Tm | BaF2–ThF4 | Glass | 2.02 | 1.56 | 1.1 | Yeh (1989) | ||
Tm | NaPO3–CaF2 | Glass | 1mol.%TmF3 | 2.03 | 1.09 | 1.17 | Gorller-Walrand (1998) | |
Tm | BIZYT fluoride | Glass | 2.05 | 1.58 | 1.12 | Guery (1988) | ||
Tm | ZBLALi | Glass | 2.09 | 1.74 | 0.91 | Gorller-Walrand (1998) | ||
Tm | ZnF2–CdF2–BaF2–LiF–AlF3–LaF3 | Glass | 2.1 | 1.5 | 1.3 | Villacampa (1991a) | ||
Tm | ZBLAN | Glass | 2%Tm | 2.21 | 1.71 | 0.92 | Gorller-Walrand (1998) | |
Tm | ZBLAN | Glass | 0.5%Tm | 2.33 | 1.44 | 0.82 | Gorller-Walrand (1998) | |
Tm | ZBLAN | Glass | 1% Tm | 2.38 | 1.82 | 0.86 | Gorller-Walrand (1998) | |
Tm | ZrBTmA | Glass | 2.39 | 1.6 | 0.89 | Oomen (1992) | ||
Tm | LiYF4 | Crystal | 2.42 | 1.28 | 0.9 | Razumova (1995) | ||
Tm | LiYF4 | Crystal | 2.43 | 1.08 | 0.67 | Dulick (1991) | ||
Tm | Y2SiO5 | Crystal | 2.43 | 1.74 | 0.66 | Li (1994) | ||
Tm | BATY | Glass | 2.46 | 1.41 | 1.13 | Gorller-Walrand (1998) | ||
Tm | PbO–PbF2 | Glass | 2.5 | 2.35 | 1.16 | Gorller-Walrand (1998) | ||
Tm | ZBLAN | Glass | 0.2 mol%Tm | 2.57 | 1.9 | 0.84 | Oomen (1992) | |
Tm | ZBLAN | Glass | 2.7 | 1.59 | 1.09 | Wettenkamp (1992) | ||
Tm | ZBLA | Glass | 2.72 | 1.82 | 0.99 | Gorller-Walrand (1998) | ||
Tm | ZrF4–BaF2–LaF3 | Glass | 0.5mol.% TmF3 | 2.73 | 1.75 | 0.96 | Tanabe and Hanada (1994) | |
Tm | HfF4–BaF2–LaF3 | Glass | 2.73 | 1.35 | 0.98 | Tanabe (1996) | ||
Tm | P2O5–AlF3–YF3–MgF2–CaF2–SrF2–BaF2–NaF | Glass | 2.75 | 2.28 | 1.18 | Peng (1995) | ||
Tm | ZBLAN | Glass | 4.32%Tm | 2.75 | 0.95 | 1.02 | Gorller-Walrand (1998) | |
Tm | LiYF4 | Crystal | 2.79 | 0.45 | 0.98 | Razumova (1995) | ||
Tm | ZBLALi | Glass | 2.8 | 1.91 | 1.01 | Sanz (1987) | ||
Tm | ZBLA | Glass | 2.8 | 1.9 | 1 | Villacampa (1991b) | ||
Tm | HfF4–BaF2–LaF3–AlF3–CsBr | Glass | 2.81 | 2.07 | 0.96 | Cases (1991) | ||
Tm | ZrF4–BaF2–BaCl2–LaF3 | Glass | 0.5mol.% TmF3 | 2.99 | 1.83 | 0.96 | Tanabe (1994) | |
Tm | germanate glass | Glass | 3.22 | 1.25 | 0.65 | Reisfeld (1975) | ||
Tm | ZrF4–BaF2–BaCl2–LaF3 | Glass | 0.5mol.% TmF3 | 3.31 | 2.03 | 0.93 | Tanabe (1994) | |
Tm | SiO2–Al2O3–Li2O–Na2O–SrO | Glass | 3.31 | 1.21 | 0.48 | Peng (1995) | ||
Tm | ZrF4-BaF2–BaCl2–LaF3 | Glass | 0.5mol.% TmF3 | 3.57 | 1.8 | 1.03 | Tanabe (1994) | |
Tm | PbO–Bi2O3–Ga2O3 | Glass | 3.59 | 0.76 | 1.27 | Heo (1995) | ||
Tm | ZrF4–BaF2–BaCl2–LaF3 | Glass | 0.5mol.% TmF3 | 3.87 | 2 | 1.02 | Tanabe and Hanada (1994) | |
Tm | GeO2–BaO–K2O | Glass | 4.05 | 1.01 | 0.28 | Peng (1995) | ||
Tm | Y2O3 | Crystal | 4.07 | 1.46 | 0.61 | Krupke (1966) | ||
Tm | GeO2–BaO–ZnO | Glass | 4.08 | 0.95 | 0.59 | Tanabe (1996) | ||
Tm | fluorophosphate glass | Glass | 4.12 | 1.47 | 0.72 | Kermanoui (1984) | ||
Tm | TeO2–BaO–ZnO | Glass | 4.23 | 0.83 | 0.74 | Tanabe (1996) | ||
Tm | MgF2–CaF2–SrF2–AlF3–Sr(PO3)2 | Glass | TmF3 | 4.27 | 2.63 | 1.22 | Seeber (1992) | |
Tm | Tm(α-picolinate) | Solution | in water | 4.82 | 7.56 | 2.89 | Bukietynska (1970) | |
Tm | P2O5–Al2O3–MgO–BaO–K2O | Glass | 4.86 | 1.68 | 0.77 | Peng (1995) | ||
Tm | Al2O3–CaO–MgO–BaO | Glass | 4.91 | 1.65 | 0.63 | Peng (1995) | ||
Tm | LiNbO3 | Crystal | 4.91 | 0.48 | 0.31 | Nunez (1993) | ||
Tm | Ga2O3–K2O–CaO–SrO–BaO | Glass | 4.98 | 1.54 | 0.6 | Peng (1995) | ||
Tm | magnesium sodium sulphate glass | Glass | 4.99 | 3.08 | 0.14 | Ratnakaram (1994) | ||
Tm | TeO2–BaO–ZnO–Y2O3 | Glass | Tm2O3 | 5.01 | 1.36 | 0.84 | Tanabe (1994) | |
Tm | tellurite glass | Glass | 5.04 | 1.36 | 1.22 | Spector (1977) | ||
Tm | LiNbO3(MgO) | Crystal | 5.3 | 0.34 | 0.42 | Nunez (1993) | ||
Tm | borate glass | Glass | 5.42 | 2.78 | 1.66 | Reisfeld (1975) | ||
Tm | Na2SO4–ZnSO4–7H2O–B2O3 | Glass | 5.81 | 7.87 | 10.75 | Rukmini (1994) | ||
Tm | phosphate glass | Glass | 5.88 | 2.88 | 0.71 | Reisfeld (1975) | ||
Tm | TeO2–BaO–ZnO–Y2O3–Er2O3 | Glass | Tm2O3 | 6.15 | 1.89 | 0.835 | Tanabe (1994) | |
Tm | germanate glass | Glass | 6.7 | 1.04 | 0.53 | Gorller-Walrand (1998) | ||
Tm | cadmium sodium sulphate glass | Glass | 6.75 | 3.49 | 0.56 | Ratnakaram (1994) | ||
Tm | (NaPO3)6–BaF2–ZnF2–20KF | Glass | 2mol% TmF3 | 7.611 | 0.396 | 6.619 | Reddy (1992a) | |
Tm | GeO2–BaO–ZnO–Y2O3 | Glass | Tm2O3 | 7.7 | 1.39 | 0.91 | Tanabe (1994) | |
Tm | potassium sodium sulphate glass | Glass | 7.83 | 5.97 | 0.22 | Ratnakaram (1994) | ||
Tm | phosphate glass | Glass | 8.08 | 3.05 | 1.66 | Spector (1977) | ||
Tm | (NaPO3)6–BaF2–ZnF2–NaF | Glass | 2mol% TmF3 | 8.52 | 0.561 | 4.721 | Reddy (1992a) | |
Tm | (NaPO3)6–BaF2–ZnF2–LiF | Glass | 2mol% TmF3 | 8.618 | 0.752 | 5.737 | Reddy (1992a) | |
Tm | K2SO4–ZnSO4·7H2O–B2O3 | Glass | 9.04 | 6.89 | 10.67 | Rukmini (1994) | ||
Tm | borate glass | Glass | 9.18 | 2.91 | 1.87 | Gorller-Walrand (1998) | ||
Tm | LiNO3–KNO3 | Melt | 10.4 | 2.8 | 1.7 | Carnall (1978) | ||
Tm | lithium sodium sulphate | Glass | 10.67 | 3.63 | 2.07 | Ratnakaram (1994) | ||
Tm | Li2SO4–ZnSO4·7H2O–B2O3 | Glass | 12.63 | 8.92 | 7.57 | Rukmini (1994) | ||
Tm | ZnSO4·7H2O–B2O3 | Glass | 12.65 | 6.99 | 10.55 | Rukmini (1994) | ||
Tm | zinc sodium sulphate | Glass | 15.95 | 3.3 | 2.46 | Ratnakaram (1994) | ||
Er | Y3Al5O12, YAG | Crystal | 0.19 | 1.68 | 0.62 | Gorller-Walrand (1998) | ||
Er | Y3Al5O12, YAG | Crystal | 20.57% Er | 0.32 | 1.19 | 0.8 | Wang (1993) | |
Er | Y3Al5O12, YAG | Crystal | 29.06% Er | 0.4 | 0.65 | 0.75 | Wang (1993) | |
Er | Y3Al5O12, YAG | Crystal | 0.45 | 0.98 | 0.62 | Kaminskii (1982) | ||
Er | Lu3Al5O12, LuAG | Crystal | 0.46 | 1.06 | 0.72 | Kaminskii (1982) | ||
Er | Y3Ga5O12 | Crystal | 0.33 | 0.26 | 0.33 | Kaminskii (1982) | ||
Er | Bi4Ge3O12 | Crystal | 1.64 | 0.51 | 0.2 | Kaminskii (1982) | ||
Er | Y2O3 | Crystal | 4.59 | 1.21 | 0.48 | Kaminskii (1982) | ||
Er | Y3Al5O12, YAG | Crystal | 17.38% Er | 0.56 | 0.99 | 0.78 | Wang (1993) | |
Er | KCaF3 | Crystal | 0.74 | 0.87 | 0.57 | Chen (1989) | ||
Er | LiErP4O12 | Crystal | 0.85 | 0.96 | 0.72 | Ryba-Romanowski (1980) | ||
Er | YAlO3 | Crystal | 0.95 | 0.58 | 0.55 | Kaminskii (1995) | ||
Er | LiYF4 | Crystal | 0.97 | 1.21 | 1.37 | Gorler-Walrand (1998) | ||
Er | BaYb2F8 | Crystal | 1.062 | 0.409 | 0.946 | Kaminskii (1996) | ||
Er | Y3Al5O12, YAG | Crystal | 0.52% Er | 1.07 | 1.61 | 1.14 | Wang (1993) | |
Er | LaF3 | Crystal | 1.16 | 1.38 | 0.88 | Weber (1972) | ||
Er | AlF3–YF3–LaF3–MgF2–CaF2–SrF2–BaF2 | Glass | 4.5mol.% ErF3 | 1.28 | 1.35 | 1.01 | Yanagita (1991) | |
Er | ZnF2–CdF2–BaF2–LiF–AlF3 | Glass | 4mol.% LaF3 | 1.3 | 1.6 | 0.9 | Villacampa (1991) | |
Er | MgCO3–Li2CO3–H3BO3 | Glass | 1mol.% Er2O3 | 1.33 | 0.39 | 0.62 | Devi (1996) | |
Er | (aquo) | (aquo) | 1.34 | 2.19 | 1.88 | Carnall (1983) | ||
Er | Y3Al5O12, YAG | Crystal | 0.79% Er | 1.43 | 1.64 | 1.28 | Wang (1993) | |
Er | LiYF4 | Crystal | 1.48 | 0.92 | 1 | Hubert (1991) | ||
Er | AlF3–MgF2–CaF2–SrF2–Sr(PO3)2 | Glass | ErF3 | 1.48 | 0.78 | 1.07 | Ledig (1990) | |
Er | (NaPO3)6–BaCl2–ZnCl2–KCl–LiCl | 2mol.% ErCl3 | 1.5 | 7.21 | 4.15 | Subramanyam (1992) | ||
Er | yttria-stabilized zirconia | Crystal | 1.5 | 0.5 | 0.22 | Merino (1991) | ||
Er | PbZnGaLa fluoride | Glass | 1.54 | 1.13 | 1.19 | Gorler-Walrand (1998) | ||
Er | Bi4Ge3O12 | Crystal | 1.66 | 0.46 | 0.21 | Kaminskii (1979) | ||
Er | ErP5O14 | Crystal | 1.68 | 2.07 | 0.98 | Ryba-Romanowski (1980) | ||
Er | ZnF2–BaF2–YF3 | Glass | 1.78 | 1.48 | 1.12 | Tanabe (1995) | ||
Er | CdCl2–CdF2–NaF–BaF2–KF | Glass | 0.15 mol% Er3+ | 1.8 | 2.62 | 1.35 | Adam (1995) | |
Er | CaCO3–Li2CO3–H3BO3 | Glass | 1 mol. % Er2O3 | 1.8 | 0.28 | 0.9 | Devi (1996) | |
Er | YAlO3 | Crystal | 1.82 | 2.38 | 1.53 | Weber (1972) | ||
Er | ZBLAK | Glass | 1.86 | 0.94 | 0.73 | Gorler-Walrand (1998) | ||
Er | BZYTZ | Glass | 1.89 | 1.54 | 0.95 | Eyal (1987) | ||
Er | LiYF4 | 1.92 | 0.26 | 1.96 | Gorler-Walrand (1998) | |||
Er | ZBLALi | Glass | 2.06 | 1.42 | 0.87 | Gorler-Walrand (1998) | ||
Er | AlF3–ZrF4–YF3–MgF2–CaF2–SrF2–BaF2–NaCl | Glass | 5 mol. % ErF3 | 2.08 | 1.29 | 1.15 | Yanagita (1991) | |
Er | InF3–BaF2–YF3 | Glass | 2.1 | 1.59 | 1.1 | Tanabe (1995) | ||
Er | ScF3–BaF2–YF3 | Glass | 2.17 | 1.45 | 1.09 | Tanabe (1995) | ||
Er | ZnF2–SrF2–NaF–BaF2–GaF3–InF3 | Glass | 1 mol. % ErF3 | 2.17 | 2.31 | 0.89 | Florez (1995) | |
Er | (NaPO3)6–BaCl2–ZnCl2–20KCl | Glass | 10mol.% ErCl3 | 2.18 | 3.97 | 4.71 | Subramanyam (1992) | |
Er | ZnF2–SrF2–NaF–BaF2–GaF3–InF3 | Glass | 3 mol. % ErF3 | 2.18 | 1.68 | 1.1 | Florez (1995) | |
Er | BaF2–ZnF2–InF3–YbF3–ThF4 | Glass | 2 mol. % ErF3 | 2.19 | 1.52 | 0.91 | Yeh (1989) | |
Er | ZBLAN | Glass | 2.2 | 1.4 | 0.91 | Gorler-Walrand (1998) | ||
Er | NaPO3–CaF2 | Glass | 1 mol. % ErF3 | 2.25 | 1.01 | 0.8 | Gorler-Walrand (1998) | |
Er | AlF3–BaF2–YF3 | Glass | 2.27 | 1.31 | 0.98 | Tanabe (1995) | ||
Er | (NaPO3)6–BaCl2–ZnCl2–NaCl | Glass | 2mol.% ErCl3 | 2.27 | 2.23 | 4.98 | Subramanyam (1992) | |
Er | GaF3–BaF2–YF3 | Glass | 2.33 | 1.51 | 1 | Tanabe (1995) | ||
Er | (NaPO3)6–BaCl2–ZnCl2–LiCl | Glass | 2mol.% ErCl3 | 2.39 | 1.43 | 0.85 | Subramanyam (1992) | |
Er | BZYTZ fluoride glass | Glass | 2.44 | 1.55 | 1.18 | Eyal (1987) | ||
Er | ZnF2–SrF2–NaF–BaF2–CaF2–InF2 | Glass | 4 mol. % ErF3 | 2.45 | 1.47 | 1.22 | Florez (1995) | |
Er | 20ZnF2–20SrF2–2NaF–16BaF2–6GaF3–34InF3 | Glass | 2 mol.% ErF3 | 2.46 | 1.63 | 1.23 | Florez (1995) | |
Er | (NaPO3)6–BaCl2–ZnCl2–KCl–LiCl | Glass | 2mol.% ErCl3 | 2.51 | 4.15 | 4.7 | Subramanyam (1992) | |
Er | SrCO3–Li2CO3–H3BO3 | Glass | 1 mol.% Er2O3 | 2.53 | 0.39 | 1.1 | Devi (1996) | |
Er | ZBLA | Glass | 2.54 | 1.39 | 0.965 | Shinn (1983) | ||
Er | LiYF4 | Crystal | 2.56 | 0.35 | 2.05 | Kaminskii (1995) | ||
Er | ZBLA | Glass | 2.59 | 1.3 | 0.85 | Gorler-Walrand (1998) | ||
Er | (NaPO3)6–BaF2–ZnF2–KF–LiF | Glass | 2mol.% ErF3 | 2.7295 | 1.6522 | 2.6806 | Reddy (1992) | |
Er | HfF4–BaF2–YF3 | Glass | 2.84 | 1.52 | 1.01 | Tanabe (1995) | ||
Er | Y2SiO5 | Crystal | 2.84 | 1.42 | 0.82 | Li (1992) | ||
Er | fluorophosphate glass | Glass | 2.88 | 1.4 | 1.27 | Yanagita (1991) | ||
Er | ZBLAN | Glass | 2.91 | 1.78 | 1 | Wetenkamp et al. (1992) | ||
Er | ZrF4–BaF2–LaF3–AlF3–NaF | Glass | 1 mol. % ErF3 | 2.91 | 1.27 | 1.11 | Zou (1993) | |
Er | P2O5–AlF3–YF3–MgF2–CaF2–SrF2–BaF2–NaF | Glass | 1 mol. % ErO1.5 | 2.91 | 1.63 | 1.26 | Zou (1993) | |
Er | ZrF2–BaF2–YF3 | Glass | 2.93 | 1.52 | 1.02 | Tanabe (1995) | ||
Er | ZBLAN | Glass | 2.97 | 1.23 | 1.17 | Yanagita (1991) | ||
Er | NTA | Solution | (1:1 in water) | 3.16 | 2.35 | 2.04 | Bukietynska and Mondry (1987) | |
Er | ErCl3 . 6H2O | Solution | in methanol | 3.2 | 3.25 | 0.8 | Keller (1982) | |
Er | HfF4–BaF2–LaF3–AlF3–CsBr | Glass | 3.2 | 1.65 | 1.23 | Cases and Chamarro (1991) | ||
Er | Li2CO3–H3BO3 | Glass | 1 mol. % Er2O3 | 3.24 | 0.92 | 0.82 | Devi (1996) | |
Er | Er(CCl3COO)3 . 2H2O | Crystal | 3.31 | 1.12 | 1.1 | Legendewicz (1991) | ||
Er | (NaPO3)6–BaF2–ZnF2–KF | Glass | 2mol.% ErF3 | 3.4001 | 5.95 | 2.4358 | Reddy (1992) | |
Er | Er2(CH3COO)6·4H2O | Crystal | 3.58 | 1.24 | 1.36 | Mondry and Bukietynska (1996) | ||
Er | CaCO3–Li2CO3–H3BO3 | Glass | 1 mol. % Er2O3 | 3.68 | 0.76 | 1.52 | Devi (1996) | |
Er | NaPO3–Er2O3 | Glass | 3.73 | 1 | 0.72 | Gorler-Walrand (1998) | ||
Er | La2S3–Al2O3 | Glass | 3.74 | 4.33 | 0.9 | Reisfeld (1982) | ||
Er | CaYAlO4 | Crystal | 3.78 | 2.52 | 1.91 | Souriau (1994) | ||
Er | NTA | Solution | (1:2 in water) | 3.84 | 2.31 | 2.16 | Bukietynska (1987) | |
Er | Ca2Al2SiO7 | Crystal | 3.85 | 1.85 | 1 | Simondi-Tesseire (1996) | ||
Er | MAL | Solution | (1:3 in water) | 3.88 | 1.95 | 2.15 | Devlin (1987) | |
Er | Y2O2S | Crystal | 3.9 | 0.91 | 0.97 | Gorler-Walrand (1998) | ||
Er | (NaPO3)6–BaCl2–ZnCl2–LiCl–NaCl | Glass | 2mol.% ErCl3 | 4.04 | 1.17 | 3.67 | Subramanyam (1992) | |
Er | NTA | Solution | (1:3) in water | 4.05 | 2.35 | 2.32 | Bukietynska (1987) | |
Er | (NaPO3)6–BaF3–ZnF3–LiF | Glass | 2mol.% ErF3 | 4.2009 | 3.2677 | 2.6256 | Reddy (1992) | |
Er | SiO2–Al2O3–(LiO0.5–NaO0.5)–SrO | Glass | 1 mol. % ErO1.5 | 4.23 | 1.04 | 0.61 | Zou (1993) | |
Er | (NaPO3)6–BaF2–ZnF2–KF–NaF | Glass | 2mol.% ErF3 | 4.5285 | 0.8512 | 2.5104 | Reddy (1992) | |
Er | Y2O3 | Crystal | 4.59 | 1.21 | 0.48 | Krupke (1966) | ||
Er | TeO2–Na2O | Glass | 1.04mol.% Er2O3 | 4.65 | 1.21 | 0.87 | Gorler-Walrand (1998) | |
Er | potassium sodium sulphate glass | Glass | 4.74 | 0.96 | 2.36 | Ratnakaram (1994) | ||
Er | phosphate glass | Glass | 4.76 | 1.14 | 0.86 | Yanagita (1991) | ||
Er | ErCl3 . 6H2O | Solution | in ethanol | 5 | 2.5 | 0.6 | Keller (1982) | |
Er | phosphate glass | Glass | 5.08 | 1.1 | 0.87 | Gorler-Walrand (1998) | ||
Er | GeO2–PbO–BaO–ZnO–K2O | Glass | 5.14 | 1.24 | 0.68 | Pan (1996) | ||
Er | GeO2–Bi2O3–PbO | Glass | 1.02 mol. % Er2O3 | 5.26 | 1.41 | 0.88 | Gorler-Walrand (1998) | |
Er | ODA | Solution | (1:3 in water) | 5.26 | 1.61 | 3.23 | Devlin (1987) | |
Er | IDA | Solution | (1:3 in water) | 5.33 | 2.17 | 2.44 | Devlin (1987) | |
Er | (NaPO3)6–BaF2–ZnF2–NaF–ErF3 | Glass | 2mol.% ErF3 | 5.3335 | 4.713 | 2.6256 | Reddy (1992) | |
Er | GeO2–PbO–TeO2–CaO | Glass | 5.44 | 1.36 | 0.97 | Pan (1996) | ||
Er | ErCl3 . 6H2O | Solution | in n-propanol | 5.5 | 2.5 | 0.7 | Keller (1982) | |
Er | AlO3–CaO–MgO–BaO | Glass | 5.6 | 1.6 | 0.61 | Zou (1993) | ||
Er | TeO2–BaO-Na2O–MgO–ZnO | Glass | 5.66 | 1.75 | 0.96 | Ryba-Romanowski (1990) | ||
Er | GaO1.5–KO0.5–CaO–SrO–BaO | Glass | 5.71 | 0.96 | 0.72 | Zou (1993) | ||
Er | (NaPO3)6–BaF2–ZnF2–NaF–LiF2 | Glass | 2mol.% ErF3 | 5.7202 | 1.6227 | 3.0597 | Reddy (1992) | |
Er | GeO2–KO0.5–BaO | Glass | 1 mol. % ErO1.5 | 5.81 | 0.85 | 0.28 | Zou (1993) | |
Er | tellurite glass | Glass | 6.05 | 1.78 | 1.07 | Yanagita (1991) | ||
Er | Pb(PO3)2 | Glass | 6.3 | 2 | 1.1 | Ingeletto (1991) | ||
Er | magnesium sodium sulphate glass | Glass | 6.39 | 3.92 | 2.22 | Ratnakaram (1994) | ||
Er | P2O5–AlO1.5–(BaO–MgO)–KO0.5 | Glass | 1 mol. % ErO1.5 | 6.65 | 1.52 | 1.11 | Zou (1993) | |
Er | CaO–Al2O3 | Glass | 1 mol% Er3+ | 6.87 | 1.5 | 0.7 | Tanabe (1993) | |
Er | K7[ErW10O35] | Crystal | 7.02 | 2.24 | 1.44 | Peacock (1973) | ||
Er | La3Ga5SiO14 | Crystal | 7.05 | 1.53 | 0.73 | Kaminskii (1990) | ||
Er | TeO2–BaO–ZnO–Y2O3–Tm2O3 | Glass | Er2O3 | 7.14 | 1.75 | 0.918 | Tanabe (1994) | |
Er | LiNbO3 | Crystal | 7.29 | 2.24 | 1.27 | Amin (1996) | ||
Er | lithium sodium sulphate glass | Glass | 7.4 | 0.98 | 2.17 | Ratnakaram (1994) | ||
Er | CaO–Al2O3 | Glass | 1 mol% Er3+ | 7.67 | 1.86 | 0.4 | Tanabe (1993) | |
Er | DPA | Solution | 1:3 in water | 7.81 | 1.67 | 3.23 | Devlin (1987) | |
Er | KY(WO4)2 | Crystal | 7.96 | 2.31 | 1.4 | Huang (1992) | ||
Er | cadmium sodium sulphate glass | Glass | 9.42 | 2.37 | 3.09 | Ratnakaram (1994) | ||
Er | Zn(PO3)2 glass | Glass | 9.9 | 1.6 | 1.8 | Ingeletto (1991) | ||
Er | zinc sodium sulphate glass | Glass | 9.99 | 2.25 | 1.77 | Ratnakaram (1994) | ||
Er | CDO | Solution | 1:3 in water | 10.45 | 2.06 | 3.41 | Devlin (1987) | |
Er | CDA | Solution | 1:3 in water | 12.03 | 2.55 | 3.56 | Devlin (1987) | |
Er | CaSO4–K2SO4–ZnSO4 | Glass | 15.18 | 1.65 | 6.69 | Subramanyam (1990) | ||
Er | LiNO3–KNO3 melt | Melt | 15.8 | 2 | 1.4 | Carnall (1978) | ||
Er | Er(α-picolinate) in water | Solution | 17.63 | 2.77 | 2.94 | Bukietynska (1970) | ||
Er | BaSO4–K2SO4–ZnSO4 | Glass | 18.37 | 1.36 | 9.39 | Subramanyam (1990) | ||
Er | MgSO4–K2SO4–ZnSO4 | Glass | 18.68 | 2.35 | 7.15 | Subramanyam (1990) | ||
Er | K2SO4 .H2O–ZnSO4-7H2O–B2O3 | Glass | 1Er2(SO4)3.7H₂O | 21.1 | 3.08 | 11.94 | Kumar (1996) | |
Er | Li2SO4 .H2O–ZnSO4-7H2O–B2O3 | Glass | 1Er2(SO4)3.7H₂O | 21.31 | 4.9 | 9.61 | Kumar (1996) | |
Er | Na2SO4 .H2O–ZnSO4-7H2O–B2O3 | Glass | 1Er2(SO4)3.7H₂O | 25.82 | 0.43 | 11.33 | Kumar (1996) | |
Er | Er(acetylacetonate)3 | Solution | in methanol | 26.11 | 1.56 | 2.09 | Gorler-Walrand (1998) | |
Er | Er(acetylacetonate)3 | Solution | in DMF | 26.4 | 2.49 | 1.09 | Gorler-Walrand (1998) | |
Er | ZnSO4.7H2O–B2O3 | Glass | 1Er2(SO4)3.7H₂O | 27.85 | 0.68 | 8.92 | Kumar (1996) | |
Er | ErCl3–(AlCl3)x | Vapor | vapor complex (400°C) | 28.5 | 4.38 | 2.09 | Carnall (1978) | |
Er | Gd2(SO4)3 .H2O–ZnSO4 .7H2O–B2O3 | Glass | 1Er2(SO4)3.7H₂O | 31.77 | 4.53 | 9.18 | Kumar (1996) | |
Er | Er(thenoyltrifluoro-acetonate)3 | Solution | in DMF | 32.36 | 2.55 | 1.96 | Gorler-Walrand (1998) | |
Er | Er(thenoyltrifluoro-acetonate)3 | Solution | in methanol | 34.72 | 1.32 | 2.7 | Gorler-Walrand (1998) | |
Er | Er(DBM)3 . H2O | Solution | 35.1 | 1.11 | 6.64 | Kirby (1981) | ||
Er | Er(DBM)3 | Solution | in methanol | 42.39 | 1.37 | 3.31 | Gorler-Walrand (1998) | |
Er | Er(DBM)3 | Solution | in DMF | 43.24 | 1.09 | 2.59 | Gorler-Walrand (1998) | |
Er | Er(DBM)3 | vapor | 46 | 2.7 | 3.7 | Gruen (1967) | ||
Er | ErBr3 | vapor | 60 | 1.47 | 1.66 | Gruen (1967) | ||
Er | ErI3 | vapor | 100 | - | - | Gruen (1967) | ||
Pm | LaF3 | Crystal | 0.5 | 1.9 | 2.2 | Leavitt (1980) | ||
Pm | LaCl3 | Crystal | 0.97 | 1.63 | 1.66 | Gorler-Walrand (1998) | ||
Pm | (aquo) | (aquo) | 1.3 | 4.36 | 3.94 | Carnall (1983) | ||
Pm | LiNO3-KNO3 | Melt | 12.5 | 3.78 | 4.14 | Carnall (1978) | ||
Tb | Na2O–SiO2 | Glass | - | 0.48 | 0.78 | Takebe (1995) | ||
Tb | K2O–CaO–SiO2 | Glass | - | 0.61 | 1.05 | Takebe (1995) | ||
Tb | NaPO3–CaF2–TbF3 | Glass | - | 0.62 | 2.78 | Gorler-Walrand (1998) | ||
Tb | Na2O–CaO–SiO2 | Glass | - | 0.68 | 1.39 | Takebe (1995) | ||
Tb | K2O–B2O3 | Glass | - | 0.73 | 1.76 | Takebe (1995) | ||
Tb | Li2O–CaO–SiO2 | Glass | - | 0.75 | 2.11 | Takebe (1995) | ||
Tb | ZBLAK | Glass | -0.2 | 3.53 | 1.88 | Gorler-Walrand (1998) | ||
Tb | ZBLALi | Glass | 0 | 2.02 | 2.3 | Gorler-Walrand (1998) | ||
Tb | ZBLA | Glass | 0.03 | 2.2 | 1.75 | Gorler-Walrand (1998) | ||
Tb | ZBLAN | Glass | 0.03 | 1.88 | 2.48 | Gorler-Walrand (1998) | ||
Tb | LaF3 | Crystal | 1.1 | 1.4 | 0.9 | Leavitt (1980) | ||
Tb | NaPO3–BaF2 | Glass | 36mol.% TbF3 | 2.75 | 3.21 | 3.36 | Duhamel-Henry (1996) | |
Tb | (aquo) | (aquo) | 2.76 | 7.95 | 2.87 | Carnall (1983) | ||
Tb | YAlO3 | Crystal | 3.25 | 7.13 | 2 | Weber (1973) | ||
Tb | ZnF2–CdF2–BaF2–LiF–AlF3–LaF3 | Glass | 1mol.% TbF3 | 4.9 | 4 | 1.6 | Gorler-Walrand (1998) | |
Tb | Li2O–B2O3 | Glass | 5.56 | 1.33 | 3.22 | Takebe (1995) | ||
Tb | Li2O–P2O5–Al2O3 | Glass | 6.44 | 1.05 | 2.21 | Takebe (1995) | ||
Tb | BaO–B2O3 | Glass | 6.72 | 0.95 | 2.81 | Takebe (1995) | ||
Tb | Na2O–P2O5–Al2O3 | Glass | 6.8 | 1.11 | 2.27 | Takebe (1995) | ||
Tb | CaO–B2O3 | Glass | 6.95 | 1.28 | 2.91 | Takebe (1995) | ||
Tb | BaO–P2O5–Al2O3 | Glass | 7.26 | 0.9 | 2.03 | Takebe (1995) | ||
Tb | CaO–B2O3 | Glass | 7.51 | 0.79 | 1.6 | Takebe (1995) | ||
Tb | MgO–P2O5–Al2O3 | Glass | 8.41 | 0.86 | 1.31 | Takebe (1995) | ||
Tb | Na2O–B2O3 | Glass | 8.82 | 0.85 | 2.8 | Takebe (1995) | ||
Tb | BaF2–InF3–ThF4–ZnF2–KF | Glass | 1mol.% TbF3 | 10.95 | 1.75 | 3.95 | Amaranath (1990) | |
Tb | BaF2–InF3–ThF4–ZnF2–LiF–KF | Glass | 1mol.% TbF3 | 12.27 | 2.04 | 4.31 | Amaranath (1990) | |
Tb | BaF2–InF3–ThF4–ZnF2–NaF | Glass | 1mol.% TbF3 | 12.32 | 1.9 | 4.32 | Amaranath (1990) | |
Tb | BaF2–InF3–ThF4–ZnF2–LiF | Glass | 1mol.% TbF3 | 13.4 | 2.15 | 4.9 | Amaranath (1990) | |
Tb | BaF2–InF3–ThF4–ZnF2–NaF–KF | Glass | 1mol.% TbF3 | 13.73 | 2.29 | 4.85 | Amaranath (1990) | |
Tb | BaF2–InF3–ThF4–ZnF2–LiF–NaF | Glass | 1mol.% TbF3 | 14.42 | 2.45 | 5.18 | Amaranath (1990) | |
Tb | LiNO3–KNO3 | Melt | 15 | 2.86 | 5.24 | Carnall (1978) | ||
Tb | TbCl3–(AlCl3)x | Vapor | Vapor Complex | 20.5 | 2.3 | 3 | Caird (1981) | |
Gd | LiYF4 | Crystal | 0.32 | - | 1.8 | Gorler-Walrand (1998) | ||
Gd | LaF3 | Crystal | 1.1 | 1.2 | 0.5 | Leavitt (1980) | ||
Gd | (aquao) | (aquao) | 1.94 | 5.27 | 4.46 | Carnall (1983) | ||
Gd | ZBLA | Glass | 2.44 | - | 2.12 | Gorler-Walrand (1998) | ||
Gd | ZBLAN | Glass | 2.49 | - | 2.3 | Gorler-Walrand (1998) | ||
Gd | ZBLALi | Glass | 2.58 | - | 2.34 | Gorler-Walrand (1998) | ||
Gd | ZBLA | Glass | 2.7 | - | 2.5 | Alonso (1988) | ||
Gd | ZBLALi | Glass | 2.7 | - | 2.5 | Alonso (1988) | ||
Gd | ZBLAN | Glass | 3.35 | - | 2.81 | Binnemans (1997) | ||
Gd | ZBLAK | Glass | 4.66 | - | 1.88 | Gorler-Walrand (1998) | ||
Gd | lanthanum borate glass | Glass | 7.27 | - | 4.11 | Verwey (1989) | ||
Eu | ZBLAN | Glass | 0.05 | 1.34 | 1.61 | Gorler-Walrand (1998) | ||
Eu | ZBLALi | Glass | 0.09 | 1.51 | 1.79 | Gorler-Walrand (1998) | ||
Eu | ZBLAK | Glass | 0.11 | 1.04 | 1.16 | Gorler-Walrand (1998) | ||
Eu | ZBLA | Glass | 0.1 | 1.54 | 1.71 | Gorler-Walrand (1998) | ||
Eu | ZBLA | Glass | 0.49 | 4.15 | 2.76 | Dejneka (1995) | ||
Eu | ZrF4–BaF2–LaF3 (ZBL) | Glass | 0.93 | 2.61 | 2.17 | Blanzat (1980) | ||
Eu | ZBANK | Glass | 1.07 | 0.52 | 0.75 | Harinath (1990) | ||
Eu | LaF3 | Crystal | 1.19 | 1.16 | 0.39 | Gorler-Walrand (1998) | ||
Eu | KY3F10 | 1.22 | 1.26 | 8.55 | Porcher (1980) | |||
Eu | ZBANLi | Glass | 1.27 | 0.61 | 0.88 | Harinath (1990) | ||
Eu | (aquo) | (aquo) | 1.46 | 6.66 | 5.4 | Carnall (1983) | ||
Eu | (aquo) | (aquo) | 1.62 | 5.65 | 5.02 | Binnemans (1997) | ||
Eu | PbO–PbF2 | Glass | 2.641 | 2.288 | 1.405 | Nachimuthu (1995) | ||
Eu | YAlO3 | Crystal | 2.66 | 6.33 | 0.8 | Weber (1973) | ||
Eu | ZBLAN | Glass | 2.89 | 3.87 | 2.88 | Binnemans (1996) | ||
Eu | NaPO3–BaF2–YF3 | Glass | 15mol.% EuF3 | 3.24 | 5.11 | 2.89 | Balda (1996b) | |
Eu | EuP5O14 | Crystal | 3.66 | 1.43 | 3.07 | Blanzat (1980) | ||
Eu | PbO–PbF2 | Glass | 3.765 | 3.086 | 1.19 | Nachimuthu (1995) | ||
Eu | NaPO3–BaF2 | Glass | 1mol.% EuF3 | 4.07 | 5.09 | 3.74 | Gorler-Walrand (1998) | |
Eu | phosphate glass | Glass | 4.12 | 4.69 | 1.83 | Blanzat (1980) | ||
Eu | InF3–BaF2–AlF3–KF | Glass | 1mol.% EuF3 | 4.9 | 0.78 | 1.6 | Annapurna (1993) | |
Eu | DPA | Solution | (1:1) in water | 5.02 | 5.65 | 5.52 | Binnemans (1997) | |
Eu | NaPO3–CaF2 | Glass | 1EuF3 | 5.12 | 5.45 | 4.12 | Gorler-Walrand (1998) | |
Eu | K7[EuW10O35] | 5.18 | 0.91 | 4.61 | Peacock (1973) | |||
Eu | InF3–BaF2–AlF3–NaF | Glass | 1mol.% EuF3 | 5.35 | 1.18 | 1.3 | Annapurna (1993) | |
Eu | NaPO3–CaF2 | Glass | 5mol.% EuF3 | 5.52 | 4.21 | 3.58 | Gorler-Walrand (1998) | |
Eu | InF3–BaF2–AlF3–LiF | Glass | 1mol.% EuF3 | 6.01 | 2.3 | 1.5 | Annapurna (1993) | |
Eu | NaPO3–BaF2–YF3 | Glass | 1mol.% EuF3 | 6.18 | 3.42 | 3.94 | Binnemans (1996) | |
Eu | Y2O3 | Crystal | 6.31 | 0.66 | <0.48 | Krupke (1966) | ||
Eu | K2O–MgO–SiO2 | Glass | 6.36 | 3.94 | 0.51 | Nageno (1994) | ||
Eu | NaPO3–MgF2 | Glass | 1mol.% EuF3 | 6.5 | 5.36 | 3.87 | Gorler-Walrand (1998) | |
Eu | K2O–MgO–SiO2 | Glass | 6.54 | 3.57 | 0.28 | Nageno (1994) | ||
Eu | NaPO3–ZnF2 | Glass | 1mol.% EuF3 | 6.75 | 6.18 | 4.23 | Gorler-Walrand (1998) | |
Eu | 25K2O–20MgO–60SiO2 | Glass | 6.86 | 4.1 | 0.55 | Nageno (1994) | ||
Eu | 5K2O–35MgO–60SiO2 | Glass | 8.65 | - | 1.66 | Nageno (1994) | ||
Eu | Eu(picNO)3 o-phen | Powder | Powder | 8.7 | 5 | - | de Sa (1994) | |
Eu | 10K2O–30MgO–60SiO2 | Glass | 8.98 | - | 1.52 | Nageno (1994) | ||
Eu | 20K2O–20MgO–60SiO2 | Glass | 9.28 | 4.81 | 0.88 | Nageno (1994) | ||
Eu | 10K2O–30MgO–60SiO2 | Glass | 9.65 | 6.68 | 1.15 | Nageno (1994) | ||
Eu | DPA | Solution | (1:3) in water | 10.5 | 5.31 | 8.32 | Binnemans (1997) | |
Eu | germanate glass | Glass | 14.83 | 1.93 | 4.67 | Gorler-Walrand (1998) | ||
Eu | Eu(picNO)3 | Powder | Powder Terpy | 22.8 | 8.3 | - | de Sa (1994) | |
Eu | LiNO3–KNO3 | Melt | Melt | 26 | - | 4.6 | Carnall (1978) | |
Eu | Eu(DBM)3·3H2O | Powder | Powder | 78.8 | - | - | Kirby (1981) | |
Sm | ZnF2–CdF2–BaF2–LiF–AlF3–LaF3 | Glass | 0.1mol.% SmF3 | 0.68 | 3.77 | 2.15 | Gorler-Walrand (1998) | |
Sm | LaF3 | Crystal | 1 | 0.5 | 1.5 | Leavitt (1980) | ||
Sm | (aquo) | (aquo) | 1.08 | 3.67 | 2.87 | Carnall (1983) | ||
Sm | HfF4–BaF2–LaF3–AlF3–CsBr | Glass | 1.44 | 2.87 | 1.44 | Cases (1991) | ||
Sm | ZBLA | Glass | 1.66 | 1.69 | 1.24 | Gorler-Walrand (1998) | ||
Sm | ZBLALi | Glass | 1.95 | 2.38 | 1.64 | Gorler-Walrand (1998) | ||
Sm | ZBLAN | Glass | 2.06 | 2.55 | 1.63 | Gorler-Walrand (1998) | ||
Sm | NaPO3–CaF2 | Glass | 1mol.% SmF3 | 2.18 | 3.8 | 2.15 | Gorler-Walrand (1998) | |
Sm | ZBLALi | Glass | 2.37 | 4.24 | 2.99 | Gorler-Walrand (1998) | ||
Sm | borate glass | Glass | 2.42 | 4.62 | 4.16 | Gorler-Walrand (1998) | ||
Sm | NaPO3–CaF2 | Glass | 5mol.% SmF3 | 2.76 | 4.11 | 2.52 | Gorler-Walrand (1998) | |
Sm | tellurite glass | Glass | 3.17 | 3.65 | 1.61 | Boehm (1979) | ||
Sm | germanate glass | Glass | 3.97 | 3.33 | 2.85 | Gorler-Walrand (1998) | ||
Sm | phosphate glass | Glass | 4.31 | 4.28 | 5.78 | Boehm (1979) | ||
Sm | ZBLAK | Glass | 4.88 | -0.35 | 1.65 | Gorler-Walrand (1998) | ||
Sm | borate glass | Glass | 6.36 | 6.02 | 3.51 | Boehm (1979) | ||
Sm | germanate glass | Glass | 6.48 | 4.98 | 3.18 | Boehm (1979) | ||
Sm | LiNO3 + KNO3 | Melt | 8.1 | 4.52 | 3.74 | Carnall (1978) | ||
Sm | ODA | Solution | (1:3 in water) | 30.17 | 4.37 | 5.96 | Gorler-Walrand (1998) | |
Sm | IDA | Solution | (1:3 in water) | 33.1 | 4.57 | 6.58 | Gorler-Walrand (1998) | |
Sm | MIDA | Solution | (1:3 in water) | 33.91 | 5.14 | 7.02 | Gorler-Walrand (1998) | |
Sm | DPA | Solution | (1:3 in water) | 44.16 | 4.28 | 5.79 | Gorler-Walrand (1998) | |
Sm | Sm(α-picolinate) | Solution | in water | 82 | 5.9 | 3.7 | Bukietynska (1970) | |
Sm | K7[SmW10O35] | 119.78 | 3.85 | 2.32 | Peacock (1973) | |||
Ho | Ho(NO3)3 .6H2O | Solution | in phtalic acid | 0.697 | 6.146 | 7.086 | Buddhudu (1991) | |
Ho | (aquo) | (aquo) | 0.791 | 3.13 | 2.86 | Carnall (1983) | ||
Ho | ZnF2–CdF2–BaF2–LiF–AlF3–LaF3 | Glass | 0.8 | 2.6 | 2 | Villacampa (1991) | ||
Ho | LaF3 | Crystal | 1.16 | 1.38 | 0.88 | Weber (1972) | ||
Ho | Ho(NO3)3 .6H2O | Solution | in benzoic acid | 1.191 | 9.04 | 7.908 | Buddhudu (1991) | |
Ho | YAG, Y3Al5O12 | Crystal | 1.2 | 5.29 | 1.48 | Gorler-Walrand (1998) | ||
Ho | NTA | Solution | (1:1) in water | 1.56 | 3.7 | 3.39 | Bukietynska (1987) | |
Ho | Ho(NO3)3 .6H2O | Solution | in salicylic acid | 1.643 | 6.273 | 8.228 | Buddhudu (1991) | |
Ho | (NaPO3)6–BaF2–ZnF2–KF | Glass | 2mol.% HoF3 | 1.66 | 2.894 | 0.632 | Reddy (1993) | |
Ho | BZYTZ fluoride glass | Glass | 1.73 | 1.89 | 1.43 | Eyal (1987) | ||
Ho | NTA | Solution | (1:3 in water) | 1.76 | 4.33 | 3.89 | Bukietynska (1987) | |
Ho | La3Ga5SiO14 | Crystal | 1.78 | 2.74 | 1.16 | Kaminskii (1990) | ||
Ho | AlF3–ZrF4–MgF2–CaF2–SrF2–BaF2–NaF–NaCl | Glass | 1.86 | 1.9 | 1.32 | Peng (1995) | ||
Ho | NTA | Solution | (1:4 in water) | 1.87 | 4.43 | 4.02 | Bukietynska (1987) | |
Ho | ZBLAN | Glass | 1.9 | 2.09 | 1.56 | Gorler-Walrand (1998) | ||
Ho | NTA | Solution | (1:2 in water) | 1.94 | 4.26 | 3.67 | Bukietynska (1987) | |
Ho | Ho³⁺:(12-crown-4) | Solution | (1:1 in acetonitrile) | 1.968 | 0.799 | 0.784 | Gorler-Walrand (1998) | |
Ho | ZBLALi | Glass | 1.99 | 2.34 | 1.7 | Gorler-Walrand (1998) | ||
Ho | P2O5–AlF3–YF3–MgF2–CaF2–SrF2–BaF2–NaF | Glass | 2.1 | 3.5 | 2.5 | Peng (1995) | ||
Ho | ZrF4–BaF2–AlF3–NaF–KF | Glass | 1mol.% HoF3 | 2.12 | 0.5 | 0.73 | Buddhudu (1988) | |
Ho | (NaPO3)6–BaCl2–ZnCl2–LiCl | Glass | 2mol.% HoCl3 | 2.14 | 9.91 | 0.27 | Subramanyam (1992) | |
Ho | ZBLAN | Glass | 2.14 | 2.22 | 2.05 | Binnemans (1996) | ||
Ho | Ho³⁺:(15-crown-15) | Solution | (1:1) in acetonitrile | 2.154 | 0.713 | 0.784 | Gorler-Walrand (1998) | |
Ho | (NaPO3)6–BaF2–ZnF2–LiF | Glass | 2mol.% HoF3 | 2.169 | 4.93 | 0.985 | Reddy (1993) | |
Ho | (NaPO3)6–BaCl2–ZnCl2–NaCl | Glass | 2mol.% HoCl3 | 2.18 | 5.92 | 0.96 | Subramanyam (1992) | |
Ho | ZBLAK | Glass | 2.2 | 1.91 | 1.38 | Gorler-Walrand (1998) | ||
Ho | NaPO3–CaF2 | Glass | 1mol.% HoF3 | 3.23 | 2.71 | 1.82 | Gorler-Walrand (1998) | |
Ho | ZBLA | Glass | 2.28 | 2.38 | 1.79 | Gorler-Walrand (1998) | ||
Ho | ZBLA | Glass | 2.28 | 2.08 | 1.73 | Tanimura (1984) | ||
Ho | ZBLAN | Glass | 2.3 | 2.3 | 1.71 | Wetenkamp (1992) | ||
Ho | (NaPO3)6–BaF2–ZnF2–LiF–NaF | Glass | 2mol.% HoF3 | 2.419 | 6.219 | 0.758 | Reddy (1993) | |
Ho | ZBLA | Glass | 2.43 | 1.67 | 1.84 | Reisfeld (1985) | ||
Ho | (NaPO3)6–BaF2–ZnF2–KF | Glass | 2mol.% HoF3 | 2.72 | 2.518 | 0.771 | Reddy (1993) | |
Ho | (NaPO3)6–BaCl2–ZnCl2–KCl | Glass | 2mol.% HoCl3 | 2.82 | 3.92 | 0.67 | Subramanyam (1992) | |
Ho | (NaPO3)6–BaCl2–ZnCl2–LiCl–KCl | Glass | 2mol.% HoCl3 | 2.9 | 5.13 | 1.32 | Subramanyam (1992) | |
Ho | (NaPO3)6–BaF2–ZnF2–NaF–KF | Glass | 2mol.% HoF3 | 3.099 | 4.363 | 0.635 | Reddy (1993) | |
Ho | (NaPO3)6–BaCl2–ZnCl2–NaCl–LiCl | Glass | 2mol.% HoCl3 | 3.11 | 7.12 | 0.77 | Subramanyam (1992) | |
Ho | DPA | Solution | (1:1, pH= 2.93) | 3.14 | 3.52 | 3.74 | Mondry (1989) | |
Ho | ZrF4–BaF2–8AlF3–NaF–KF | Glass | 1mol.% HoF3 | 3.15 | 0.74 | 1.09 | Buddhudu (1988) | |
Ho | (NaPO3)6–BaF2–ZnF2–KF–LiF | Glass | 2mol.% HoF3 | 3.195 | 3.549 | 0.457 | Reddy (1993) | |
Ho | GeO2–BaO–K2O | Glass | 3.3 | 1.14 | 0.14 | Peng (1995) | ||
Ho | HfF4–BaF2–LaF3–AlF3–CsBr | Glass | 3.3 | 2.22 | 1.93 | Cases(1991) | ||
Ho | P2O5–Al2O3–MgO–BaO–K2O | Glass | 3.33 | 3.01 | 0.61 | Peng (1995) | ||
Ho | K7[HoW10O35] | 3.52 | 2.33 | 2.6 | Peacock (1973) | |||
Ho | SiO2–Al2O3–Li2O–Na2O–SrO | Glass | 3.6 | 2.3 | 0.65 | Peng (1995) | ||
Ho | (NaPO3)6–BaCl2–ZnCl2–NaCl–KCl | Glass | 2mol.% HoCl3 | 3.64 | 3.36 | 0.84 | Subramanyam (1992) | |
Ho | ODA | Solution | (1:3 in water) | 3.88 | 4.02 | 4.24 | Devlin (1988) | |
Ho | Li2O–CaO–SiO2 | Glass | 4.03 | 2.47 | 1.07 | Takebe (1995) | ||
Ho | ZrF4–BaF2–AlF3–NaF–KF | Glass | 1mol.% HoF3 | 4.09 | 0.97 | 1.41 | Buddhudu (1988) | |
Ho | IDA | Solution | (1:3 in water) | 4.09 | 5.01 | 4.18 | Devlin (1988) | |
Ho | Na2O–SiO2 | Glass | 4.24 | 1.09 | 0.47 | Takebe (1995) | ||
Ho | Na2O–CaO–SiO2 | Glass | 4.44 | 1.51 | 0.71 | Takebe (1995) | ||
Ho | Li2O–B2O3 | Glass | 4.56 | 3.14 | 1.78 | Takebe (1995) | ||
Ho | Ho(α-picolinate) | Solution | in water | 4.62 | 4.07 | 3.88 | Bukietynska(1970) | |
Ho | Ho(NO3)3 . 6H2O | Solution | in anthrolinic acid | 4.628 | 1.116 | 7.978 | Buddhudu (1991) | |
Ho | MIDA | Solution | (1:3 in water) | 4.64 | 3.76 | 3.32 | Devlin (1988) | |
Ho | PbO–Bi2O3–Ga2O3 | Glass | 4.77 | 2.18 | 1.22 | Shin (1995) | ||
Ho | Al2O3–CaO–MgO–BaO | Glass | 4.9 | 2.5 | 0.68 | Peng (1995) | ||
Ho | CaO–B2O3 | Glass | 4.9 | 3.29 | 1.74 | Takebe (1995) | ||
Ho | Li2O–P2O5–Al2O3 | Glass | 4.92 | 2.28 | 1.54 | Takebe (1995) | ||
Ho | BaO–B2O3 | Glass | 4.96 | 2.99 | 1.61 | Takebe (1995) | ||
Ho | DPA | Solution | (1:2, pH=3.17) | 5.14 | 3.84 | 3.71 | Mondry (1989) | |
Ho | K2O–CaO–SiO2 | Glass | 5.19 | 1.35 | 0.61 | Takebe (1995) | ||
Ho | K2O–B2O3 | Glass | 5.29 | 1.4 | 0.78 | Takebe (1995) | ||
Ho | 30Na2O–70B2O3 | Glass | 5.3 | 2.52 | 1.53 | Takebe (1995) | ||
Ho | 30Na2O–60P2O5–10Al2O3 | Glass | 5.31 | 2.62 | 1.62 | Takebe (1995) | ||
Ho | ZrF4–BaF2–AlF3–LiF–NaF | Glass | 1HoF3 | 5.32 | 1.26 | 1.84 | Buddhudu (1988) | |
Ho | DPA | Solution | 1:4, pH=3.33 | 5.35 | 3.97 | 4.28 | Mondry (1989) | |
Ho | BaO–P2O5–Al2O3 | 5.36 | 2.39 | 1.33 | Takebe (1995) | |||
Ho | NaPO3 | Glass | 5.6 | 2.72 | 1.87 | Reisfeld (1976) | ||
Ho | Ho³⁺ in Ga₂O₃–K₂O–CaO–SrO–BaO glass | Glass | 5.7 | 3.1 | 0.37 | Peng (1995) | ||
Ho | CaO–60P₂O₅–10Al₂O₃ glass | Glass | 6.23 | 1.56 | 1.21 | Takebe (1995) | ||
Ho | DPA | (1:3 in water) | 6.39 | 4.03 | 4.11 | Devlin (1988) | ||
Ho | MgO–P2O5–Al2O3 | 6.58 | 1.57 | 1.09 | Takebe (1995) | |||
Ho | ZrF4–BaF2–AlF3–LiF–NaF | Glass | 1mol.% HoF3 | 6.77 | 1.31 | 1.87 | Buddhudu (1988) | |
Ho | CaO–Li2O–B2O3 | Glass | 6.83 | 3.15 | 2.53 | Reisfeld (1976) | ||
Ho | Na2O–TeO2 | Glass | 6.92 | 2.81 | 1.42 | Reisfeld(1976) | ||
Ho | Ge30As10Se60 | Glass | 6.98 | 2.53 | 0.78 | Shin (1995) | ||
Ho | DPA | Solution | (1:4, pH=7.10) | 7.72 | 3.8 | 5.32 | Mondry (1989) | |
Ho | DPA | Solution | (1:4, pH=11.17) | 7.54 | 3.91 | 5.25 | Mondry (1989) | |
Ho | La2S3–Al2S3 | Glass | 8.1 | 3.8 | 1.4 | Gorler-Walrand (1998) | ||
Ho | ZrF4–BaF2–AlF3–LiF–NaF | Glass | 1mol.% HoF3 | 8.13 | 1.58 | 2.24 | Buddhudu (1988) | |
Ho | Na3[Ho(dpa)3] NaClO4 . 10H2O | Crystal | 9.27 | 3.49 | 4.55 | Mondry (1989) | ||
Ho | B2O3–Na2O–AlF3 | Glass | 1mol.% HoF3 | 9.934 | 22.989 | 3.096 | Gorler-Walrand (1998) | |
Ho | CDA | Solution | (1:3 in water) | 10.11 | 5.07 | 4.81 | Devlin (1988) | |
Ho | CDO | Solution | (1:3 in water) | 11.09 | 5.17 | 4.86 | Devlin (1988) | |
Ho | B2O3–Na2O–LiF | Glass | 1mol.% HoF3 | 11.92 | 17.025 | 2.964 | Gorler-Walrand (1998) | |
Ho | B2O3–Na2O–NaF | Glass | 1mol.% HoF3 | 12.174 | 18.895 | 4.745 | Gorler-Walrand (1998) | |
Ho | B2O3–Na2O–NaF–AlF3 | Glass | 1mol.% HoF3 | 12.861 | 12.77 | 7.141 | Gorler-Walrand (1998) | |
Ho | B2O3–Na2O–LiF–AlF3 | Glass | 1mol.% HoF3 | 12.989 | 10.206 | 8.16 | Gorler-Walrand (1998) | |
Ho | LiNO3–KNO3 | Melt | Melt | 16.4 | 3.6 | 2.3 | Carnall (1978) | |
Ho | Li2SO4.H2O–ZnSO4.7H2O–B2O3 | Glass | 1mol.% Ho2(SO4)3 . 8H2O | 18.95 | 7.25 | 10.45 | Rukmini (1995) | |
Ho | Na2SO4.H2O–ZnSO4.7H2O–B2O3 | Glass | 1mol.% Ho2(SO4)3 . 8H2O | 20.32 | 10.34 | 11.31 | Rukmini (1995) | |
Ho | K2SO4.H2O–ZnSO4.7H2O–B2O3 | Glass | 1mol.% Ho2(SO4)3 . 8H2O | 21.92 | 7.45 | 11.23 | Rukmini (1995) | |
Ho | ZnSO4.7H2O–B2O3 | Glass | 1mol.% Ho2(SO4)3 . 8H2O | 22.42 | 5.19 | 12.33 | Rukmini (1995) | |
Ho | Ho(DBM)3 . H2O | Powder | Powder | 42.8 | <0.01 | 1.95 | Kirby (1981) | |
Dy | K7[DyW10O35] | -23.01 | 4.95 | 3.28 | Peacock (1973) | |||
Dy | (aquo) | (aquo) | 0.584 | 3.54 | 3.9 | Carnall (1983) | ||
Dy | LaF3 | Crystal | 1.1 | 1.4 | 0.9 | Xu (1984) | ||
Dy | ODA | Solution | (1:3 in water) | 1.03 | 0.271 | 1.211 | Gorler-Walrand (1998) | |
Dy | MIDA | Solution | (1:3 in water) | 1.292 | -0.333 | 1.277 | Gorler-Walrand (1998) | |
Dy | IDA | Solution | (1:3 in water) | 1.298 | 0.177 | 1.192 | Gorler-Walrand (1998) | |
Dy | Dy2(C5H8NO4)2(ClO4)4 .9H2O | 1.35 | 2.67 | 3.82 | Csoreg (1989) | |||
Dy | Dy(α-picolinate) | Solution | in water | 1.37 | 3.44 | 4.7 | Bukietynska (1970) | |
Dy | ZnF2–CdF2–BaF2–LiF–AlF3–LaF3 | Glass | 1.38 | 1.05 | 2.35 | Cases (1991) | ||
Dy | Na2O–P2O5 | Glass | 1.46 | 1.16 | 1.97 | Hormadaly (1979) | ||
Dy | DPA | Solution | (1:3 in water) | 1.767 | 0.735 | 1.402 | Gorler-Walrand (1998) | |
Dy | ZBLAN | Glass | 1.86 | 1.42 | 2.37 | Wetenkamp (1992) | ||
Dy | DyCl₃·xH₂O | Solution | in CH₃OH | 2.02 | 2.69 | 2.67 | Legendziewicz (1984) | |
Dy | ZBLALi | Glass | 2.6 | 1.13 | 1.91 | Gorler-Walrand (1998) | ||
Dy | ZBLA | Glass | 2.65 | 1.29 | 1.72 | Gorler-Walrand (1998) | ||
Dy | ZBLALi | Glass | 2.7 | 1.8 | 2 | Gorler-Walrand (1998) | ||
Dy | ZBLAN | Glass | 3.03 | 1.32 | 2.06 | Gorler-Walrand (1998) | ||
Dy | Dy³⁺ in POCl3/ZrCl4 | Solution | in POCl3/ZrCl4 | 3.09 | 2.23 | 3.33 | Bukietynska (1981) | |
Dy | ZBLAK | Glass | 3.13 | 1.14 | 1.87 | Gorler-Walrand (1998) | ||
Dy | HfF4–BaF2–LaF3–AlF3–CsBr | Glass | 3.12 | 2.07 | 2.48 | Cases (1991) | ||
Dy | BaO–TeO2 | Glass | 3.2 | 1.35 | 2.47 | Hormadaly (1979) | ||
Dy | ZBLA | Glass | 3.22 | 1.35 | 2.38 | Adam (1988) | ||
Dy | NaPO3–CaF2 | Glass | 1mol.% DyF3 | 3.63 | 2.03 | 1.89 | Gorler-Walrand (1998) | |
Dy | Na2O–TeO2 | Glass | 3.7 | 1.15 | 2.22 | Hormadaly (1979) | ||
Dy | DyCl3 .xH2O | Solution | in C₂H₅OH | 4.27 | 2.2 | 1.74 | Legendziewicz (1984) | |
Dy | ZnO–TeO2 | Glass | 4.28 | 1.32 | 2.53 | Hormadaly (1979) | ||
Dy | Li2O–CaO–SiO2 | Glass | 5.87 | 1.94 | 1.22 | Takebe (1995) | ||
Dy | Li2O–B2O3 | Glass | 5.9 | 1.82 | 2.02 | Takebe (1995) | ||
Dy | CaO–B2O3 | Glass | 5.99 | 2.01 | 1.96 | Takebe (1995) | ||
Dy | Na2O–SiO2 | Glass | 6.04 | 0.9 | 0.24 | Takebe (1995) | ||
Dy | Li2O–P2O5–Al2O3 | Glass | 6.19 | 1.8 | 1.5 | Takebe (1995) | ||
Dy | Na2O–CaO–SiO2 | Glass | 6.42 | 1.46 | 0.65 | Takebe (1995) | ||
Dy | BaO–B2O3 | Glass | 6.44 | 1.66 | 1.84 | Takebe (1995) | ||
Dy | K2O–B2O3 | Glass | 6.62 | 0.99 | 0.63 | Takebe (1995) | ||
Dy | Dy2(CH3COO)6 .4H2O | Crystal | 6.69 | 1.89 | 3.67 | Mondry (1996) | ||
Dy | Na2O–P2O5–Al2O3 | Glass | 6.7 | 1.98 | 1.73 | Takebe (1995) | ||
Dy | K2O–CaO–SiO2 | Glass | 6.81 | 1.39 | 0.43 | Takebe (1995) | ||
Dy | Na2O–B2O3 | Glass | 6.85 | 1.64 | 1.61 | Takebe (1995) | ||
Dy | BaO–P2O5–Al2O3 | Glass | 7.11 | 1.75 | 1.47 | Takebe (1995) | ||
Dy | DyCl3 .xH2O | Solution | in C₂H₅OH | 7.39 | 2.42 | 2 | Legendziewicz (1984) | |
Dy | CaO–P2O5–Al2O3 | Glass | 8.13 | 1.48 | 1.21 | Takebe (1995) | ||
Dy | MgO–P2O5–Al2O3 | Glass | 8.21 | 1.38 | 1.14 | Takebe (1995) | ||
Dy | LiNbO3 | Crystal | 9.57 | 2.63 | 2.52 | Malinowski (1996) | ||
Dy | Ge30As10S60 | Glass | 10.53 | 3.17 | 1.17 | Heo (1996) | ||
Dy | Ge25Ga5S70 | Glass | 11.86 | 4 | 1.47 | Heo (1996) | ||
Dy | Ga2S3–La2S3 | Glass | 11.3 | 1 | 1.3 | Hewak (1994b) | ||
Dy | Ge25Ga5O70 | Glass | 11.9 | 3.58 | 2.17 | Wei (1994) | ||
Dy | LiNO3–KNO3 melt | Melt | melt | 14.4 | 1.4 | 3.16 | Carnall (1978) | |
Pr | Y3Al5O12, YAG | Crystal | -1.34 | 12.2 | 8.27 | Malinowski (1990) | ||
Pr | ZBLA | Glass | -1 | 4.4 | 7.8 | Eyal (1985) | ||
Pr | ZBLA | Glass | -0.76 | 4.91 | 8.54 | Gorler-Walrand (1998) | ||
Pr | ZBLALi | Glass | -0.65 | 5.54 | 8.95 | Gorler-Walrand (1998) | ||
Pr | Li2CO3-H3BO3 | Glass | -0.461 | 5.854 | 7.477 | Gorler-Walrand (1998) | ||
Pr | ZBLAN | Glass | -0.37 | 5.36 | 0.54 | Gorler-Walrand (1998) | ||
Pr | InF3-BaF2-ThF4-ZnF2-KF | Glass | 1mol.% PrF3 | -0.37 | 13.19 | 3.61 | Amaranath (1990) | |
Pr | InF3-BaF2-ThF4-ZnF2-NaF-KF | Glass | 1mol.% PrF3 | -0.11 | 14.56 | 4.41 | Amaranath (1990) | |
Pr | CaO-B2O3 | Glass | -0.1 | 4.75 | 5.12 | Takebe (1995) | ||
Pr | LiYF4 | Crystal | 0 | 8.07 | 7.32 | Adam (1985) | ||
Pr | ZnO-TeO2 | Glass | 0 | 9.96 | 21.47 | Kanoun (1990) | ||
Pr | PbO-PbF2 | Glass | 0.02 | 7.88 | 4.81 | Gorler-Walrand (1998) | ||
Pr | ZBLAN | Glass | 0.04 | 4.99 | 13.06 | Binnemans (1997) | ||
Pr | Li2O-B2O3 | Glass | 0.1 | 4.71 | 5.28 | Takebe (1995) | ||
Pr | LaF3 | Crystal | 0.12 | 1.77 | 4.78 | Gorler-Walrand (1998) | ||
Pr | HfF4-BaF2-LaF3-AlF3-CsBr | Glass | 0.212 | 5.82 | 6.68 | Cases (1991) | ||
Pr | ZBLA | Glass | 0.24 | 4.51 | 5.37 | Eyal (1985) | ||
Pr | lithium sodium sulphate | Glass | 0.27 | 12.54 | 9.01 | Ratnakaram (1994) | ||
Pr | KPrP4O12 | Crystal | 0.34 | 4.36 | 1.81 | Kornienko (1990) | ||
Pr | SrCO3-Li2CO3-H3BO3 | Glass | 0.357 | 5.091 | 6.335 | Gorler-Walrand (1998) | ||
Pr | ZBLYAN | Glass | 0.47 | 3.73 | 4.09 | Gorler-Walrand (1998) | ||
Pr | BaO-B2O3 | Glass | 0.5 | 4.98 | 5 | Takebe (1995) | ||
Pr | InF3-BaF2-SrF2-PbF2-ZnF2 | Glass | PrF3 | 0.523 | 3.82 | 4.92 | Gorler-Walrand (1998) | |
Pr | InF3-BaF2-SrF2-CdF2 | Glass | PrF3 | 0.601 | 4.18 | 5.07 | Gorler-Walrand (1998) | |
Pr | ZnF2-CdF2-BaF2-LiF-AlF3-LaF3 | Glass | 0.5mol.% PrF3 | 0.72 | 4.8 | 7.93 | Gorler-Walrand (1998) | |
Pr | BIGaZLuTZrPb | Glass | 0.73 | 4.74 | 4.97 | Adam (1991) | ||
Pr | Li2O-2B2O3 | Glass | 0.77 | 3.84 | 3.58 | Hormadaly (1979) | ||
Pr | Na2O-2B2O3 | Glass | 0.77 | 4.13 | 3.07 | Hormadaly (1979) | ||
Pr | ZBLAN | Glass | 0.84 | 4.79 | 9.13 | Wetenkamp (1992) | ||
Pr | ZnF2-SrF2-BaF2-InF3 | Glass | 0.85 | 4.13 | 12.33 | Gorler-Walrand (1998) | ||
Pr | ZBLAN | Glass | 0.94 | 6.54 | 3.84 | Binnemans (1997) | ||
Pr | potassium sodium sulphate | Glass | 0.97 | 3.32 | 3.15 | Ratnakaram (1994) | ||
Pr | Na2O-B2O3 | Glass | 0.98 | 4.76 | 4.86 | Takebe (1995) | ||
Pr | (NaPO3)6-BaCl2-ZnCl2-LiCl-NaCl | Glass | 2mol.% PrCl3 | 1.056 | 0.965 | 0.912 | Subramanyam (1992) | |
Pr | InF3-BaF2-ThF4-ZnF2-NaF | Glass | 1mol.% PrF3 | 1.11 | 13.98 | 3.44 | Amaranath (1990b) | |
Pr | magnesium sodium sulphate | Glass | 1.16 | 5.6 | 3.62 | Ratnakaram (1994) | ||
Pr | (NaPO3)6-BaCl2-ZnCl2-KCl-LiCl | Glass | 2mol.% PrCl3 | 1.233 | 1.684 | 0.473 | Subramanyam (1992) | |
Pr | (NaPO3)6-BaCl2-ZnCl2-NaCl | Glass | 2mol.% PrCl3 | 1.317 | 2.082 | 0.714 | Subramanyam (1992) | |
Pr | AlF3-SrF2-CaF2-MgF2-P2O5 | Glass | 3mol.% PrF3 | 1.4 | 4.2 | 5.2 | Seeber (1995) | |
Pr | ZBLAN | Glass | 1.431 | 4.221 | 4.872 | Gorler-Walrand (1998) | ||
Pr | ZBLAN | Glass | 1.46 | 4.89 | 4.85 | Remillieux (1996) | ||
Pr | (NaPO3)6-BaCl2-ZnCl2-KCl | Glass | 2mol.% PrCl3 | 1.549 | 1.344 | 1.034 | Subramanyam (1992) | |
Pr | (NaPO3)6-BaCl2-ZnCl2-NaCl-KCl | Glass | 2mol.% PrCl3 | 1.557 | 1.044 | 1.102 | Subramanyam (1992) | |
Pr | ZrF2-BaF2-LaF3 | Glass | 1.56 | 5.81 | 5.45 | Hirao et al. (1994) | ||
Pr | ZBLAN | Glass | 1.6 | 5.06 | 4.79 | Adam et al. (1991) | ||
Pr | MgCO3-Li2CO3-H3BO3 | Glass | 1.796 | 3.575 | 6.915 | Gorler-Walrand (1998) | ||
Pr | AlF3-SrF2-CaF2-MgF2-P2O5 | Glass | 10mol.% PrF3 | 1.8 | 4.7 | 5.2 | Seeber (1995) | |
Pr | LiPrP4O12 | Crystal | 1.82 | 2.83 | 6.54 | Mazurak (1984) | ||
Pr | YAlO3 | Crystal | 2 | 6 | 7 | Gorler-Walrand (1998) | ||
Pr | Na2O-P2O5-Al2O3 | Glass | 2.06 | 6.41 | 5.61 | Takebe (1995) | ||
Pr | K2O-B2O3 | Glass | 2.14 | 2.91 | 1.67 | Hormadaly (1979) | ||
Pr | InF3-BaF2-ThF4-ZnF2-KF-LiF | Glass | 1mol.% PrF3 | 2.2 | 17.27 | 6.93 | Amaranath (1990b) | |
Pr | K2O-B2O3 | Glass | 2.33 | 4.65 | 3.84 | Takebe (1995) | ||
Pr | Li2O-P2O5-Al2O3 | Glass | 2.41 | 5.89 | 5.6 | Takebe (1995) | ||
Pr | ZBLAN | Glass | 2.5 | 5.4 | 6 | Seeber (1995) | ||
Pr | cadmium sodium sulphate | Glass | 2.57 | 3 | 3.57 | Ratnakaram (1994) | ||
Pr | ZnO-TeO2 | Glass | 2.59 | 7.26 | 5.45 | Hormadaly (1979) | ||
Pr | Li2O-CaO-SiO2 | Glass | 2.69 | 6.01 | 4.7 | Takebe (1995) | ||
Pr | AlF3-SrF2-CaF2-MgF2-P2O5 | Glass | 20 mol% PrF3 | 2.7 | 5.3 | 5 | Seeber (1995) | |
Pr | Na2O-TeO2 | Glass | 2.83 | 6.5 | 4.6 | Hormadaly (1979) | ||
Pr | ZBLAN | Glass | 2.9 | 6.4 | 5.5 | Simons (1995) | ||
Pr | MgCl2 | Solution | saturated solution | 2.95 | 3.48 | 2.43 | Lakshman (1982) | |
Pr | BaCO3-Li2CO3-H3BO3 | Glass | 2.991 | 6.713 | 11.868 | Gorler-Walrand (1998) | ||
Pr | fluoroindate glass | Glass | 3.2 | 4.5 | 6.5 | Seeber (1995) | ||
Pr | zinc sodium sulphate | Glass | 3.44 | 15.19 | 10.22 | Ratnakaram (1994) | ||
Pr | BaPO3-P2O5-Al2O3 | Glass | 3.53 | 5.66 | 4.77 | Takebe (1995) | ||
Pr | NaPO3-CaF2 | Glass | 1mol.% PrF3 | 3.67 | 5.75 | 5.59 | Gorler-Walrand (1998) | |
Pr | Na2O-CaO-SiO2 | Glass | 3.91 | 5.72 | 3.82 | Takebe (1995) | ||
Pr | (NaPO3)6-BaCl2-ZnCl2-LiCl | Glass | 2mol.% PrCl3 | 4.382 | 1.867 | 1.281 | Subramanyam (1992b) | |
Pr | Na2O-SiO2 | Glass | 4.81 | 4.71 | 3.01 | Takebe (1995) | ||
Pr | BaO-TeO2 | Glass | 4.95 | 6.46 | 5.44 | Hormadaly (1979) | ||
Pr | K2O-CaO-SiO2 | Glass | 5.16 | 5.21 | 2.5 | Takebe (1995) | ||
Pr | CaO-P2O5-Al2O3 | Glass | 5.28 | 5.2 | 4.34 | Takebe (1995) | ||
Pr | InF3-BaF2-ThF4-ZnF2-LiF | Glass | 1mol.% PrF3 | 5.64 | 13.32 | 4.15 | Amaranath (1990) | |
Pr | ZBLAK | Glass | 6.1 | 0.36 | 6.57 | Gorler-Walrand (1998) | ||
Pr | CaCl2 | Solution | 6.11 | 1.3 | 3.85 | Lakshman (1982) | ||
Pr | MgO-P2O5-Al2O3 | Glass | 6.44 | 4.52 | 3.95 | Takebe (1995) | ||
Pr | ZBLA | Glass | 6.68 | 5.05 | 6.92 | Adam (1985) | ||
Pr | La3Ga5SiO14 | Crystal | 6.89 | 2.76 | 6.24 | Kaminskii (1990) | ||
Pr | NH4Cl | Solution | saturated solution | 7.04 | 2.57 | 2.78 | Lakshman (1982) | |
Pr | CdCl2 | Solution | saturated solution | 7.12 | 3.33 | 3.05 | Lakshman (1982) | |
Pr | Ga2S3-La2S3 | Glass | 7.3 | 6.2 | 3.9 | Hewak (1994) | ||
Pr | CaCO3-Li2CO3-H3BO3 | Glass | 7.361 | 1.031 | 12.105 | Gorler-Walrand (1998) | ||
Pr | LiNO3-KNO3 | Melt | 8.63 | 6.3 | 6.48 | Carnall (1978) | ||
Pr | PrCl3 | Solution | in water | 9.25 | 3.56 | 2.18 | Lakshman (1982) | |
Pr | Pr(benzoylacetonate)3 | Solution | in DMF | 9.42 | 12.83 | 20.81 | Tandon (1970) | |
Pr | Pr(acetylacetonate)3 | Solution | in DMF | 9.57 | 12.9 | 12.98 | Tandon (1970) | |
Pr | GeS2-Ga2S3 | Glass | 9.6 | 15.4 | 4.4 | Simons (1995) | ||
Pr | Zn(PO3)2 | Glass | 10 | 2 | 7 | Ingeletto (1991) | ||
Pr | GeS2-Ga2S3 | Glass | 11.6 | 5.6 | 6 | Simons (1995) | ||
Pr | GeS2.5-Ga2S3 | Glass | 12.8 | 4.3 | 7.7 | Wei (1995) | ||
Pr | GeS2-Ga2S3 | Glass | 13.2 | 8.6 | 6.1 | Simons (1995) | ||
Pr | Pb(PO3)2 | Glass | 14.8 | 9.7 | 26.9 | Ingeletto (1991) | ||
Pr | Y2O3 | Crystal | 17.21 | 19.8 | 4.88 | Krupke (1966) | ||
Pr | Pr(thenoyltrifluoroacetonate)3 | Solution | in DMF | 23.12 | 16.09 | 22.69 | Tandon (1970) | |
Pr | K7[PrW10O35] | 26.97 | 5.1 | 36.94 | Peacock (1973) | |||
Pr | (aquo) | (aquo) | 28 | 5.89 | 32.2 | Carnall (1983) | ||
Pr | Pr(alpha-picolinate)3 | solution | in water | 46 | 7 | 39.5 | Bukietynska (1970) | |
Pr | Pr(acetylacetonate)3 | solution | in methanol | 51.79 | 14.38 | 18.35 | Tandon (1970) | |
Pr | (NaPO3)6-BaF2-ZnF2-KF | Glass | 2mol.% PrF3 | 57 | 1.23 | 2.81 | Reddy (1991) | |
Pr | Pr(benzoylacetonate)3 | Solution | in methanol | 62.6 | 15.16 | 20.61 | Tandon (1970) | |
Pr | Pr(thenoyltrifluoroacetonate)3 | Solution | in methanol | 70.54 | 13.22 | 22.79 | Tandon (1970) | |
Pr | (NaPO3)6-BaF2-ZnF2-NaF | Glass | 2mol.% PrF3 | 88 | 2.16 | 3.74 | Reddy (1991) | |
Pr | (NaPO3)6-BaF2-ZnF2-LiF-NaF | Glass | 2mol.% PrF3 | 97 | 1.73 | 4.03 | Reddy (1991) | |
Pr | (NaPO3)6-BaF2-ZnF2-LiF | Glass | 2mol.% PrF3 | 117 | 1.91 | 4.19 | Reddy (1991) | |
Pr | Sr_xBa_1-xNb2O6 | Crystal | 145.731 | 0.6821 | 1.5881 | Zhang (1994) | ||
Pr | (NaPO3)6-BaF2-ZnF2-NaF-KF | Glass | 2mol.% PrF3 | 160 | 2.3 | 2.94 | Reddy (1991) | |
Pr | (NaPO3)6-BaF2-ZnF2-LiF-KF | Glass | 2mol.% PrF3 | 188 | 2.23 | 4.05 | Reddy (1991) | |
Nd | Lu3Sc2Ga3O12 | Crystal | 0.082 | 2.844 | 3.137 | Kaminskii et al. (1994) | ||
Nd | BeF2–KF | Glass | 2mol.% NdF3 | 0.1 | 2.7 | 3.2 | Stokowski(1981) | |
Nd | BeF2–AlF3–CaF2–LiF | Glass | 2mol.% NdF3 | 0.1 | 3.7 | 3.8 | Stokowski(1981) | |
Nd | BeF2–AlF3–CaF2–NaF | Glass | 2mol.% NdF3 | 0.1 | 3.7 | 4.3 | Stokowski(1981) | |
Nd | BeF2–KF–CsF | Glass | 2mol.% NdF3 | 0.1 | 4 | 5 | Stokowski(1981) | |
Nd | BeF2–KF | Glass | 1mol.% NdF3 | 0.1 | 4.4 | 5.3 | Stokowski(1981) | |
Nd | BeF2–KF–CaF2–AlF3 | Glass | 2mol.% NdF3 | 0.2 | 3.9 | 4.6 | Stokowski(1981) | |
Nd | BeF2–KF–LiF | Glass | 2mol.% NdF3 | 0.2 | 3.9 | 5.1 | Stokowski(1981) | |
Nd | YAG, Y3Al5O12 | Crystal | 0.2 | 2.7 | 5 | Krupke (1971) | ||
Nd | Y3Sc2Al3O12 | Crystal | 0.23 | 2.87 | 4.78 | Allik (1990) | ||
Nd | SrF2 | Crystal | 0.24 | 1.24 | 1.72 | Payne (1991) | ||
Nd | BaF2 | Crystal | 0.25 | 0.41 | 0.43 | Payne (1991) | ||
Nd | LiYF4 | Crystal | 0.25 | 4.09 | 4.83 | Kaminskii (1994) | ||
Nd | BeF2–KF–KCl | Glass | 2mol.% NdF3 | 0.3 | 3 | 3.7 | Stokowski (1981) | |
Nd | BeF2–KF–CaF2–AlF3 | Glass | 2mol.% NdF3 | 0.3 | 3.4 | 4.3 | Stokowski et al. (1981) | |
Nd | LaF3: | Crystal | 0.35 | 2.6 | 2.5 | Krupke (1966) | ||
Nd | LiYF4 | Crystal | 0.362 | 4.02 | 4.84 | Ryan (1992) | ||
Nd | Y3Al5O12, YAG | Crystal | 0.37 | 2.29 | 5.97 | Kaminski (1974) | ||
Nd | BeF2–NaF–MgF2–CaF2–AlF3 | Glass | 1.5mol.% NdF3 | 0.4 | 2.8 | 3.5 | Stokowski (1981) | |
Nd | BeF2–AlF3–CaF2–RbF | Glass | 2mol.% NdF3 | 0.4 | 3.9 | 4.8 | Stokowski (1981) | |
Nd | NdGaO3 | Crystal | 0.46 | 3.6 | 2.6 | Orera (1995) | ||
Nd | (CaF2, LaF3) | Crystal | 0.48 | 2.53 | 3.74 | Payne (1991) | ||
Nd | BeF2–KF–AlF3–CaF2 | Glass | 2mol.% NdF3 | 0.5 | 3.1 | 4 | Stokowski (1981) | |
Nd | BeF2–AlF3–KF–MgF2 | Glass | 2mol.% NdF3 | 0.5 | 3.5 | 4.6 | Stokowski (1981) | |
Nd | BeF2–AlF3–KF–SrF2 | Glass | 2mol.% NdF3 | 0.5 | 3.5 | 4.6 | Stokowski (1981) | |
Nd | AlF3–CaF2–BaF2 | Glass | 1mol.% NdF3 | 0.6 | 3.7 | 4.1 | Tesar (1992) | |
Nd | Y2SiO5 | Crystal | 0.67 | 6.19 | 2.71 | Gorler-Walrand (1998) | ||
Nd | PbF2–MnF2–GaF3 | Glass | 1mol.% NdF3 | 0.7 | 3.7 | 3.8 | Tesar (1992) | |
Nd | K7[NdW10O53] | 0.77 | 5.56 | 7.06 | Peacock (1973) | |||
Nd | Ca2Ga2SiO7 | Crystal | 0.82 | 4.41 | 6.44 | Gorler-Walrand (1998) | ||
Nd | La3Lu2Ga5O12 | Crystal | 0.84 | 2.64 | 2.61 | Allik (1988) | ||
Nd | KYF4 | Crystal | 0.85 | 2.38 | 3.93 | Kaminskii (1994) | ||
Nd | KYF4 | Crystal | 0.86 | 2.39 | 3.93 | Allik (1993) | ||
Nd | CaF2 | Crystal | 0.87 | 3.44 | 9.47 | Sardar (1993) | ||
Nd | ZnF2–BaF2–AlF3–YF3–ThF4 | Glass | 1mol.% NdF3 | 0.9 | 3.8 | 4 | Tesar (1992) | |
Nd | GdGaGe2O7 | Crystal | 0.907 | 2.773 | 5.981 | Kaminskii (1987) | ||
Nd | LiKYF5 | Crystal | 0.92 | 3.21 | 4.26 | Kaminskii (1994) | ||
Nd | AlF3–ZrF4–MgF2–CaF2–SrF2–BaF2–YF3 | Glass | NdF3 | 1 | 3.6 | 4.2 | Tesar (1992) | |
Nd | AlF3–BeF2–MgF2–CaF2–SrF2–BaF2–YF3–LaF3 | Glass | NdF3 | 1 | 3.7 | 4.1 | Tesar (1992) | |
Nd | BeF2–AlF3–KF–CaF2 | Glass | 2mol.% NdF3 | 1 | 4.7 | 5.9 | Stokowski (1981) | |
Nd | YSZ | 1.1 | 1.24 | 1.23 | Gorler-Walrand (1998) | |||
Nd | AlF3–BeF2–CaF2–BaF2 | Glass | 1mol.% NdF3 | 1.1 | 3.2 | 3.9 | Tesar (1992) | |
Nd | magnesium sodium sulphate glass | Glass | 1.12 | 2.81 | 3.67 | Ratnakaram (1994) | ||
Nd | Nd(ClO4)3 | Solution | in DMF | 1.2 | 8.9 | 8.4 | Bünzli (1984) | |
Nd | Nd(ClO4)3 | Solution | in CH3CN | 1.2 | 7.7 | 9.8 | Bünzli (1984) | |
Nd | AlF3–BeF2–MgF2–CaF2–SrF2–BaF2–YF3 | Glass | NdF3 | 1.2 | 3.7 | 4.3 | Tesar (1992) | |
Nd | CLAP | Glass | 1.2 | 3.9 | 4.7 | Tesar (1992) | ||
Nd | ZBLA | Glass | 1.23 | 3.37 | 3.2 | Gorller-Walrand (1998) | ||
Nd | YAlO3 | Crystal | 1.24 | 4.68 | 5.85 | Weber (1971) | ||
Nd | Ba0.25Mg2.75Y2Ge3O12 | Crystal | 1.25 | 3.23 | 3.26 | Sardar (1995) | ||
Nd | BIGaZYTZrPb fluoride glass | Glass | 1.26 | 2.74 | 4.01 | Adam (1991) | ||
Nd | BIGaZLuTMn fluoride | Glass | 1.26 | 2.58 | 4.08 | Azkargorta (1994) | ||
Nd | LuAlO3 | Crystal | 1.28 | 4.45 | 4.88 | Kaminskii (1991) | ||
Nd | ZBLALi | Glass | 1.28 | 3.91 | 3.78 | Gorller-Walrand (1998) | ||
Nd | Al(PO3)3–BaF2–MgF2 | Glass | 1mol.% Nd2O3 | 1.3 | 4.7 | 5.1 | Stokowski (1981) | |
Nd | BIGaZYTZr fluoride glass | Glass | 1.31 | 2.71 | 4.01 | Elejalde (1992) | ||
Nd | ZrF4–AlF3–YF3–SrF2–BaF2–ZnF2 | Glass | 1mol.% NdF3 | 1.38 | 2.58 | 3.86 | Binnemans (1998) | |
Nd | BeF2 | Glass | 2mol.% NdF3 | 1.4 | 2.9 | 3.6 | Stokowski (1981) | |
Nd | ZnF2–CaF2–BaF2–LiF–AlF3–LaF3 | Glass | 1.4 | 2.77 | 5.77 | Cases (1991) | ||
Nd | ZBLAK | Glass | 1.4 | 3.477 | 3.08 | Gorller-Walrand (1998) | ||
Nd | AlF3–BaF2–YF3–ThF4 | Glass | 1mol.% NdF3 | 1.5 | 3.3 | 3.6 | Tesar (1992) | |
Nd | PZG fluoride glass | Glass | 1.53 | 3.19 | 4.93 | Balda (1994) | ||
Nd | ZBLAN | Glass | 1.54 | 3.66 | 3.5 | Gorller-Walrand (1998) | ||
Nd | BeF2–MgF2–CaF2–BaF2–AlF3 | Glass | 1mol.% NdF3 | 1.6 | 3.6 | 3.9 | Tesar (1992) | |
Nd | Al(PO3)3–AlF3–YF3–MgF2–CaF2–SrF2–BaF2 | Glass | 1mol.% NdF3 | 1.6 | 3.8 | 4.5 | Stokowski (1981) | |
Nd | ZBT | Glass | 1.7 | 4 | 4.2 | Tesar (1992) | ||
Nd | ZBAT | Glass | 1.7 | 3.8 | 3.8 | Tesar (1992) | ||
Nd | ZF2–BaF2–AlF3–LaF3–NaF | Glass | 1mol.% NdF3 | 1.76 | 3.08 | 3.67 | Binnemans (1996) | |
Nd | HfF4–BaF2–ThF4 | Glass | 1mol.% NdF3 | 1.8 | 4 | 3.9 | Tesar (1992) | |
Nd | HfF4–BaF2–AlF3–ThF4 | Glass | 1mol.% NdF3 | 1.8 | 4.3 | 4.3 | Tesar (1992) | |
Nd | Al(PO3)3–AlF3–MgF2–CaF2–SrF2–BaF2 | Glass | 1mol.% NdF3 | 1.8 | 3.2 | 4.5 | Stokowski (1981) | |
Nd | Ba(PO3)2–AlF3–BaF2–MgF2–CaF2–SrF2–NaF | Glass | 1mol.% NdF3 | 1.8 | 3.8 | 4.6 | Stokowski (1981) | |
Nd | Al(PO3)3–AlF3–NaF–MgF2–CaF2–SrF2–BaF2 | Glass | 1mol.% NdF3 | 1.8 | 3.8 | 4.9 | Stokowski (1981) | |
Nd | MgF2–AlF3–LiF–NaPO3 | Glass | 0.5mol.% Nd2O3 | 1.8 | 5.3 | 5.6 | Stokowski (1981) | |
Nd | Ca3Ga2Ge4O14 | Crystal | 1.88 | 3.65 | 5.65 | Kaminskii et al. (1984) | ||
Nd | ZBALBe | Glass | 1.9 | 3.5 | 3.7 | Tesar (1992) | ||
Nd | HfF4–BaF2–LaF3–ThF4 | Glass | 1mol.% NdF3 | 1.9 | 3.7 | 4.2 | Tesar (1992) | |
Nd | ZrF4–BaF2–NdF3 | Glass | 1.95 | 3.65 | 4.17 | Lucas (1978) | ||
Nd | trifluoroacetate | Solution | in water | 1.96 | 2.34 | 5.38 | Surana (1980) | |
Nd | ZrF4–BaF2–LaF3, ZBL | Glass | 1mol.% NdF3 | 2 | 3.9 | 3.8 | Tesar (1992) | |
Nd | ZrF4–BaF2–LaF3–AlF3, ZBLA | Glass | 1mol.% NdF3 | 2 | 3.6 | 3.8 | Tesar (1992) | |
Nd | ZBLAN | Glass | 2 | 3.9 | 4.3 | Tesar (1992) | ||
Nd | ZrF4–BaF2–AlF3–YF3, ZBAY | Glass | 1mol.% NdF3 | 2 | 3.7 | 4 | Tesar (1992) | |
Nd | HfF4–BaF2–AlF3–LaF3, HBLA | Glass | 1mol.% NdF3 | 2 | 3.7 | 4 | Tesar (1992) | |
Nd | NaF–LiF–Mg(PO3)2– glass | Glass | 1mol.% Nd2O3 | 2 | 4.7 | 5.3 | Stokowski (1981) | |
Nd | (NaPO3)6–BaCl2–ZnCl2–LiCl–KCl | Glass | 2mol.% NdCl3 | 2.02 | 1.41 | 4.21 | Subramanyam (1992) | |
Nd | BaCO3–Li2CO3–H3BO3 | Glass | 1mol.% Nd2O3 | 2.02 | 10.62 | 4.94 | Devi and Jayasankar (1995) | |
Nd | LaGaO3 | Crystal | 2.1 | 2.4 | 2.3 | Orera (1995) | ||
Nd | ZrF4–BaF2–ThF4, HBT | Glass | 1mol.% NdF3 | 2.1 | 3.6 | 4.1 | Tesar (1992) | |
Nd | ZBLAN | Glass | 2.1 | 3.71 | 4.62 | Wetenkamp (1992) | ||
Nd | (NaPO3)6–BaCl2–ZnCl2–NaCl–KCl | Glass | 2mol.% NdCl3 | 2.19 | 1.61 | 4.2 | Subramanyam (1992) | |
Nd | ZBLAN | Glass | 2.2 | 2.82 | 3.94 | Adam (1991) | ||
Nd | Mg(PO3)2–AlF3–MgF2–CaF2–SrF2–BaF2 | Glass | 1mol.% NdF3 | 2.2 | 4.2 | 4.9 | Stokowski (1981) | |
Nd | ZnCl2–KI glass | Glass | 2.2 | 8.1 | 5 | Weber (1982) | ||
Nd | ZrF4–BaF2–LiF–ThF4, ZBTLi | Glass | 1mol.% NdF3 | 2.2 | 3.3 | 4.8 | Tesar (1992) | |
Nd | HfF4–ZrF4–CsF–BaF2–YF3–LaF3–ThF4, HZBYLTCS | Glass | 1mol.% NdF3 | 2.2 | 3.8 | 4.3 | Tesar (1992) | |
Nd | (aquo) | (aquo) | 2.25 | 4.08 | 9.47 | Carnall (1983) | ||
Nd | Sr3Ga2Ge4O14 | 2.32 | 1.63 | 4.74 | Kaminskii (1984) | |||
Nd | Al(PO3)3–BaF2–CaF2–MgF2–AlF3 | Glass | 1mol.% Nd2O3 | 2.33 | 2.78 | 4.43 | Balda (1996) | |
Nd | HfF4–BaF2–LaF3–AlF3–CsBr | Glass | 2.36 | 4.48 | 4.72 | Cases (1991) | ||
Nd | 75NaPO3–24SrF2 | Glass | 1mol.% NdF3 | 2.39 | 4.02 | 6.1 | Binnemans (1998) | |
Nd | HfF4–CsF–BaF2–YF3–LaF3–ThF4, HBYLTCs | Glass | 1mol.% NdF3 | 2.4 | 4.1 | 4.3 | Tesar (1992) | |
Nd | La3Ga5SiO14 | Crystal | 2.4 | 4.6 | 3.4 | Kaminski (1983) | ||
Nd | NaPO3–ZnCl2 | Glass | 0.1mol.% Nd2O3 | 2.4 | 5.9 | 6.2 | Weber (1981) | |
Nd | NaPO3–BaF2 | Glass | 1mol.% NdF3 | 2.41 | 3.27 | 5.19 | Binnemans (1998) | |
Nd | trichloroacetate | Solution | in water | 2.42 | 1.55 | 5.88 | Surana (1980) | |
Nd | ODA | Solution | (1:3 in water) | 2.42 | 3.92 | 8.56 | Devlin (1988) | |
Nd | Al(PO3)3–LiF–NaF | Glass | 1mol.% Nd2O3 | 2.5 | 5.3 | 5.6 | Stokowski (1981) | |
Nd | La2O3–PbO–TeO2–SiO2–B2O3–Ba3Y3WO9 | Glass | 2.54 | 0.97 | 1.88 | Bullock (1997) | ||
Nd | Pb(PO3)2 | Glass | 2.6 | 3.5 | 4.3 | Gorller-Walrand (1998) | ||
Nd | Al(PO3)3–LiF–Li2O–BaF2 | Glass | 1mol.% Nd2O3 | 2.6 | 5.4 | 5.7 | Stokowski (1981) | |
Nd | potassium sodium sulphate | Glass | 2.61 | 4.57 | 5.45 | Ratnakaram (1994) | ||
Nd | ZBLAN | Glass | 2.66 | 3.05 | 4.08 | Balda (1994) | ||
Nd | tribromoacetate | Solution | in water | 2.66 | 1.26 | 5.64 | Surana (1980) | |
Nd | LiF–Al(PO3)3 | Glass | 0.5mol.% NdF3 | 2.7 | 4.8 | 5.1 | Stokowski (1981) | |
Nd | NaPO3–CaF2 | Glass | 1mol.% NdF3 | 2.78 | 4.16 | 5.56 | Binnemans (1998) | |
Nd | (NaPO3)6–BaCl2–ZnCl2–LiCl–10NaCl | Glass | 2mol.% NdCl3 | 2.85 | 0.3 | 4.49 | Subramanyam (1992) | |
Nd | InF3–BaF2–AlF3–KF | Glass | 1mol.% NdF3 | 2.86 | 1.61 | 1.3 | Annapurna et al. (1992) | |
Nd | (NaPO3)6–BaCl2–ZnCl2–KCl | Glass | 2mol.% NdCl3 | 2.87 | 0.49 | 3.97 | Subramanyam (1992) | |
Nd | P2O5–K2O–MgO | Glass | 0.58mol.% Nd2O3 | 2.9 | 4.6 | 5.1 | Stokowski (1981) | |
Nd | (NaPO3)6–BaCl2–ZnCl2–LiCl | Glass | 2mol.% NdCl3 | 2.95 | 0.4 | 4.06 | Subramanyam (1992) | |
Nd | SiO2–Li2O–MgO–Al2O3 | Glass | 0.34mol.% Nd2O3 | 3 | 4.6 | 4.5 | Stokowski (1981) | |
Nd | dichloroacetate | Solution | in water | 3.01 | 2.42 | 5.89 | Surana (1980) | |
Nd | (NaPO3)6–BaCl2–ZnCl2–NaCl | Glass | 2mol.% NdCl3 | 3.09 | 0.86 | 4.24 | Subramanyam (1992) | |
Nd | ZBAN | Glass | 3.09 | 3.65 | 5.74 | Petrin (1991) | ||
Nd | TeO2–P2O5 | Glass | 0.27mol.% NdF3 | 3.1 | 4 | 3.9 | Stokowski (1981) | |
Nd | SiO2–Al2O3–Li2O–CaO–CeO2 | Glass | 0.8mol.% Nd2O3 | 3.1 | 4.6 | 5.1 | Gorller-Walrand (1998) | |
Nd | monofluoroacetate | Solution | in water | 3.1 | 1.45 | 5.62 | Surana (1980) | |
Nd | NaPO3–NaF | Glass | 1mol.% NdF3 | 3.19 | 3.73 | 5.55 | Binnemans (1998) | |
Nd | NaPO3–CdF2 | Glass | 1mol.% NdF3 | 3.19 | 3.88 | 5.73 | Binnemans (1998) | |
Nd | (α-picolinate) | Solution | in water | 3.2 | 10.4 | 10.3 | Bukietynska (1970) | |
Nd | dibromoacetate | Solution | in water | 3.21 | 1.62 | 5.78 | Surana (1980) | |
Nd | DPA | Solution | (1:1 in water) | 3.26 | 4.27 | 9.67 | Mondry (1995) | |
Nd | MIDA | Solution | (1:3 in water) | 3.29 | 4.62 | 8.36 | Devlin (1988) | |
Nd | P2O5–Li2O–Al2O3–Na2O–CaO | Glass | 0.7mol.% Nd2O3 | 3.3 | 4.7 | 5.4 | Gorller-Walrand (1998) | |
Nd | P2O5–K2O–BaO | Glass | 0.53mol.% Nd2O3 | 3.3 | 5 | 5.6 | Gorller-Walrand (1998) | |
Nd | SiO2–Li2O–BaO | Glass | 0.3mol.% Nd2O3 | 3.3 | 3.5 | 4 | Gorller-Walrand (1998) | |
Nd | IDA | Solution | (1:3 in water) | 3.31 | 5.08 | 9.3 | Devlin (1988) | |
Nd | Li2O–P2O5–CaO–Al2O3 | Glass | 0.7mol.% Nd2O3 | 3.4 | 4.8 | 5.4 | Gorller-Walrand (1998) | |
Nd | P2O5–Li2O–CaO–Al2O3 | Glass | 0.7mol.% Nd2O3 | 3.4 | 4.4-4.6 | 5.1-5.3 | Gorller-Walrand (1998) | |
Nd | Li6Y5(BO3)3 | Crystal | 3.44 | 3.99 | 4.67 | Huang (1992) | ||
Nd | NaPO3–LiF | Glass | 1mol.% NdF3 | 3.44 | 4.14 | 6.28 | Binnemans (1998) | |
Nd | monoiodoacetate | Solution | in water | 3.5 | 2.07 | 6.17 | Surana (1980) | |
Nd | TeO2–Nb2O5 | Glass | 1.55mol.% Nd2O3 | 3.5 | 3.5 | 3.5 | Stokowski (1981) | |
Nd | P2O5–Li2O–SiO2–Al2O3–CaO | Glass | 0.7mol.% Nd2O3 | 3.5 | 4.4 | 5.2 | Gorller-Walrand (1998) | |
Nd | NaPO3–ZnCl2 | Glass | 0.1mol.% Nd2O3 | 3.5 | 5.4 | 6.6 | Weber (1981) | |
Nd | TeO2–ZnO | Glass | 1mol.% Nd2O3 | 3.6 | 4.6 | 4.3 | Stokowski (1981) | |
Nd | TeO2–Li2O | Glass | 1mol.% Nd2O3 | 3.6 | 4.9 | 4.6 | Stokowski (1981) | |
Nd | P2O5–Li2O–Al2O3–CaO | Glass | 0.7mol.% Nd2O3 | 3.6 | 4.7 | 5.4 | Gorller-Walrand (1998) | |
Nd | SiO2–Li2O | Glass | 0.5mol.% Nd2O3 | 3.6 | 3.9 | 4.3 | Gorller-Walrand (1998) | |
Nd | GeO2–Li2O | Glass | 0.57mol.% Nd2O3 | 3.6 | 3.6 | 4.1 | Stokowski (1981) | |
Nd | NaPO3–KF | Glass | 1mol.% NdF3 | 3.61 | 3.81 | 5.83 | Binnemans (1998) | |
Nd | Na2O–P2O5–Al2O3 | Glass | 3.62 | 4.73 | 5.68 | Nageno (1993) | ||
Nd | Li2O–CaO–SiO2 | Glass | 3.63 | 4.21 | 4.94 | Takebe (1995) | ||
Nd | Na2O–P2O5–CaO–Al2O3 | Glass | 0.7mol.% Nd2O3 | 3.7 | 4 | 4.4 | Gorller-Walrand (1998) | |
Nd | monochloroacetate | Solution | in water | 3.7 | 1.79 | 5.18 | Surana (1980) | |
Nd | SiO2–Na2O–BaO | 0.3mol.% Nd2O3 | 3.7 | 3.2 | 3.6 | Gorller-Walrand (1998) | ||
Nd | CaO–Al2O3–Na2O–SrO | 0.5mol% Nd2O3 | 3.71 | 5.03 | 2.9 | Uhlmann (1994) | ||
Nd | Li2O–P2O5–Al2O3 | Glass | 3.71 | 4.7 | 5.15 | Takebe (1995) | ||
Nd | P2O5–Bi2O3–Ga2O3 | Glass | 3.72 | 4.48 | 4.33 | Takebe (1996) | ||
Nd | NaPO3–ZnF2 | Glass | 1mol.% NdF3 | 3.75 | 4.05 | 5.99 | Binnemans (1998) | |
Nd | ZrF4–BaF2–AlF3–KF | Glass | 1mol.% NdF3 | 3.75 | 5.45 | 8.95 | Hanumanthu (1991) | |
Nd | NaPO3–ZnO | Glass | 0.5mol.% Nd2O3 | 3.76 | 3.27 | 5.23 | Binnemans (1998) | |
Nd | NaPO3 | Glass | 3.8 | 5.3 | 6 | Gorller-Walrand (1998) | ||
Nd | Na2O–P2O5–Al2O3 | Glass | 3.82 | 4.74 | 5.53 | Takebe (1995) | ||
Nd | PbO–Ga2O3 | Glass | 3.84 | 3.87 | 4.07 | Takebe (1996) | ||
Nd | PbO–Bi2O3–Ga2O3 | Glass | 3.88 | 4.24 | 4.3 | Takebe (1996) | ||
Nd | P2O5–Bi2O3–Ga2O3 | Glass | 3.89 | 4.07 | 4.31 | Takebe (1996) | ||
Nd | P2O5–K2O–ZnO | Glass | 1mol.% Nd2O3 | 3.9 | 4.8 | 5.5 | Gorller-Walrand (1998) | |
Nd | SiO2–BaO–K2O | Glass | 1.19mol.% Nd2O3 | 3.9 | 2.3 | 2.2 | Gorller-Walrand (1998) | |
Nd | Cd(PO3)2 | Glass | 3.9 | 4.2 | 4.6 | Gorller-Walrand (1998) | ||
Nd | BaO–P2O5–La2O3 | Glass | 0.3mol.% Nd2O3 | 3.9 | 4.3 | 5.1 | Gorller-Walrand (1998) | |
Nd | Nd3+ monobromoacetate | Solution | in water | 3.9 | 2 | 5.72 | Surana (1980) | |
Nd | DPA | Solution | (1:2 in water) | 3.92 | 4.32 | 10.37 | Mondry (1995) | |
Nd | PbO–Bi2O3–Ga2O3 | Glass | 3.94 | 4.09 | 4.31 | Takebe (1996) | ||
Nd | CaO–Al2O3–Na2O | Glass | 0.5mol.% Nd2O3 | 3.95 | 4.81 | 3.2 | Uhlmann (1994) | |
Nd | (NdCl6)3+ | Solution | in acetonitrile | 3.95 | 1.23 | 0.72 | Henrie (1977) | |
Nd | K2O–P2O5–CaO–Al2O3 | Glass | 0.7mol.% Nd2O3 | 4 | 5.1 | 5.9 | Gorller-Walrand (1998) | |
Nd | Ba(PO3)2 | Glass | 4 | 5.4 | 5.6 | Weber (1981) | ||
Nd | SiO2–Na2O | Glass | 0.3mol.% Nd2O3 | 4 | 3.2 | 3 | Gorller-Walrand (1998) | |
Nd | TeO2–BaO | Glass | 1mol.% Nd2O3 | 4 | 5.1 | 4.8 | Stokowski (1981) | |
Nd | 65SiO2–35Na2O | Glass | 0.3mol.% Nd2O3 | 4.1 | 3.2 | 3.3 | Gorller-Walrand (1998) | |
Nd | 70SiO2–30Na2O | Glass | 0.3mol.% Nd2O3 | 4.1 | 3.2 | 3.3 | Gorller-Walrand (1998) | |
Nd | TeO2–Na2O | Glass | 1mol.% Nd2O3 | 4.1 | 4.8 | 4.6 | Stokowski (1981) | |
Nd | SiO2–Na2O | Glass | 0.3mol.% Nd2O3 | 4.2 | 2.8 | 2.8 | Gorller-Walrand (1998) | |
Nd | SiO2–K2O–BaO | Glass | 0.3mol.% Nd2O3 | 4.2 | 2.5 | 2.7 | Gorller-Walrand (1998) | |
Nd | SiO2–Na2O | Glass | 0.5mol.% Nd2O3 | 4.2 | 3.3 | 3.1 | Gorller-Walrand (1998) | |
Nd | Bi2O3–CdO–SiO2 | Glass | 0.5mol.% Nd2O3 | 4.2 | 4 | 4.9 | Gorller-Walrand (1998) | |
Nd | Li2O–B2O3 | Glass | 4.2 | 3.89 | 4.74 | Takebe (1995) | ||
Nd | ZnO–TeO2 | Glass | 4.24 | 0.88 | 7.05 | Kanoun (1990) | ||
Nd | SiO2–K2O | Glass | 0.41mol.% Nd2O3 | 4.3 | 1.7 | 1.8 | Gorller-Walrand (1998) | |
Nd | SiO2–CaO–Na2O–K2O–BaO | Glass | 0.19mol.% Nd2O3 | 4.3 | 2.7 | 2.9 | Gorller-Walrand (1998) | |
Nd | Sr(PO3)2 | Glass | 4.3 | 4.3 | 5 | Weber (1981) | ||
Nd | SrO–P2O5–La2O3 | Glass | 0.3mol.% Nd2O3 | 4.3 | 4.4 | 5 | Gorller-Walrand (1998) | |
Nd | CaO–B2O3 | Glass | 4.36 | 3.74 | 4.64 | Takebe (1995) | ||
Nd | BaO–P2O5–Al2O3 | Glass | 4.37 | 4.05 | 4.82 | Takebe (1995) | ||
Nd | SiO2–Na2O | Glass | 0.37mol.% Nd2O3 | 4.4 | 2.6 | 3 | Gorller-Walrand (1998) | |
Nd | SiO2–K2O–SrO | Glass | 0.3mol.% Nd2O3 | 4.4 | 2.8 | 2.9 | Gorller-Walrand (1998) | |
Nd | SiO2–K2O–BaO | Glass | 4.4 | 2.5 | 2.6 | Gorller-Walrand (1998) | ||
Nd | Rb2O–P2O5–CaO–Al2O3 | Glass | 0.7mol.% Nd2O3 | 4.4 | 5.5 | 6.2 | Gorller-Walrand (1998) | |
Nd | CaO–Al2O3–Na2O–BaO | Glass | 0.5mol.% Nd2O3 | 4.46 | 5.18 | 2.73 | Uhlmann (1994) | |
Nd | Ca(PO3)2 | Glass | 4.5 | 4.8 | 4.9 | Weber (1981) | ||
Nd | SiO2–K2O | Glass | 0.5mol.% Nd2O3 | 4.5 | 2.2 | 2 | Gorller-Walrand (1998) | |
Nd | NaPO3 | Glass | 1mol.% NdF3 | 4.52 | 3.94 | 5.93 | Binnemans (1998) | |
Nd | La(PO3)3 | Glass | 0.5mol.% Nd2O3 | 4.6 | 3.9 | 4 | Gorller-Walrand (1998) | |
Nd | Al(PO3)3 | Glass | 0.5mol.% Nd2O3 | 4.6 | 4.1 | 4.3 | Gorller-Walrand (1998) | |
Nd | Na2O–CaO–SiO2 | Glass | 4.64 | 3.81 | 4.17 | Takebe (1995) | ||
Nd | BaO–B2O3 | Glass | 4.65 | 3.56 | 4.74 | Takebe (1995) | ||
Nd | CaO–P2O5–La2O3 | Glass | 0.3mol.% Nd2O3 | 4.7 | 4.2 | 4.7 | Gorller-Walrand (1998) | |
Nd | TeO2–Cs2O | Glass | 1mol.% Nd2O3 | 4.7 | 4.9 | 4.4 | Stokowski (1981) | |
Nd | DPA | Solution | (1:3 in water) | 4.7 | 4.78 | 11.31 | Devlin (1988) | |
Nd | Nd(PO3)3 | Glass | 4.8 | 3.2 | 3.7 | Weber (1981) | ||
Nd | SiO2–K2O–CaO | Glass | 0.3mol.% Nd2O3 | 4.8 | 3.2 | 3.1 | Gorller-Walrand (1998) | |
Nd | TeO2–K2O | Glass | 1mol.% Nd2O3 | 4.8 | 5.3 | 5 | Stokowski (1981) | |
Nd | Na2O–SiO2 | Glass | 4.83 | 3.07 | 3.37 | Takebe (1995) | ||
Nd | CaO–Al2O3 | Glass | 0.5mol.% Nd2O3 | 4.87 | 5.5 | 3.42 | Uhlmann (1994) | |
Nd | SiO2–Na2O | Glass | 0.48mol.% Nd2O3 | 4.9 | 2.9 | 2.9 | Gorller-Walrand (1998) | |
Nd | Na2O–B2O3 | Glass | 4.91 | 3.28 | 4.51 | Takebe (1995) | ||
Nd | K2O–B2O3 | Glass | 4.94 | 3.1 | 3.42 | Takebe (1995) | ||
Nd | Zn(PO3)2 | Glass | 5.1 | 4.4 | 4.7 | Gorller-Walrand (1998) | ||
Nd | Ta2O5–SiO2–B2O3–BaO | Glass | 1mol.% Nd2O3 | 5.1 | 4.1 | 4.1 | Stokowski (1981) | |
Nd | TeO2–Rb2O | Glass | 1mol.% Nd2O3 | 5.1 | 5.1 | 4.4 | Stokowski (1981) | |
Nd | SiO2–Na2O–BaO–ZnO | Glass | 0.5mol.% Nd2O3 | 5.1 | 3.2 | 3.6 | Gorller-Walrand (1998) | |
Nd | P2O5–MgO–MnO | Glass | 1.16mol.% Nd2O3 | 5.1 | 3.7 | 4.2 | Gorller-Walrand (1998) | |
Nd | SiO2–BaO–TiO2 | Glass | 0.73mol.% Nd2O3 | 5.2 | 3.9 | 3.2 | Gorller-Walrand (1998) | |
Nd | sodium Beta''-alumina | 5.19 | 0.973 | 0.971 | Alfrey (1988) | |||
Nd | K2O–CaO–SiO2 | Glass | 5.23 | 3.1 | 3.14 | Takebe (1995) | ||
Nd | Nd3+ in 30CaO–60P2O5–10Al2O3 glass | Glass | 5.27 | 3.69 | 4.31 | Takebe (1995) | ||
Nd | Mg(PO3)2 | Glass | 5.3 | 4.7 | 4.3 | Weber (1981) | ||
Nd | Bi2O3–CdO–SiO2 | Glass | 0.56mol.% Nd2O3 | 5.4 | 5.1 | 5.9 | Gorller-Walrand (1998) | |
Nd | NdBr3 | Solution | in acetonitrile | 5.46 | 3.15 | 1.08 | Henrie (1977) | |
Nd | P2O5–MgO–As2O3 | Glass | 0.78mol.% Nd2O3 | 5.7 | 4.1 | 4.5 | Gorller-Walrand (1998) | |
Nd | TeO2–K2O | Glass | 1mol.% Nd2O3 | 5.7 | 5 | 4.7 | Stokowski (1981) | |
Nd | BiCl3–KCl | Glass | 5.7 | 6.6 | 4.4 | Weber (1982) | ||
Nd | MgO–P2O5–Al2O3 | Glass | 5.72 | 3.69 | 4.31 | Takebe (1995) | ||
Nd | H3BO3–Na2CO3–LiF | Glass | 1mol.% NdF3 | 5.758 | 1.702 | 5.484 | Ratnakaram (1996) | |
Nd | SiO2–K2O–MgO | Glass | 0.3mol.% Nd2O3 | 5.8 | 3.3 | 3.1 | Gorller-Walrand (1998) | |
Nd | SiO2–Na2O | Glass | 0.41mol.% Nd2O3 | 5.8 | 3.4 | 3 | Gorller-Walrand (1998) | |
Nd | YVO4 | Crystal | 5.88 | 4.08 | 5.11 | Lomheim (1978) | ||
Nd | 40MgO–55P2O5–4.7La2O3 | Glass | 0.3mol.% Nd2O3 | 6 | 4 | 4.7 | Gorller-Walrand (1998) | |
Nd | SiO2 | Glass | 0.09mol.% Nd2O3 | 6 | 4.7 | 4.1 | Gorller-Walrand (1998) | |
Nd | Al(PO3)3–Zn2P2O7 | Glass | 1mol.% Nd2O3 | 6.1 | 3.3 | 3.8 | Gorller-Walrand (1998) | |
Nd | P2O5–Al2O3 | Glass | 0.395mol.% Nd2O3 | 6.2 | 3.6 | 4.2 | Gorller-Walrand (1998) | |
Nd | Al(PO3)3 | Glass | 6.3 | 4 | 4.6 | Gorller-Walrand (1998) | ||
Nd | MgCO3–Li2CO3–H3BO3 | Glass | 1mol.% Nd2O3 | 6.3 | 33.17 | 9.51 | Devi (1995) | |
Nd | P2O5 | Glass | 16.67mol.% Nd2O3 | 6.4 | 4.7 | 5.3 | Gorller-Walrand (1998) | |
Nd | SrCO3–Li2CO3–H3BO3 | Glass | 1mol.% Nd2O3 | 6.52 | 5 | 6.16 | Devi (1995) | |
Nd | InF3–BaF2-AlF3–NaF | Glass | 1mol.% NdF3 | 6.56 | 2.31 | 2.81 | Annapurna (1992) | |
Nd | cadmium sodium sulphate | Glass | 6.61 | 3.97 | 6.65 | Ratnakaram (1994) | ||
Nd | Ga2S3–La2S3 | Glass | Nd2S3 | 6.65 | 4.39 | 4.67 | Bornstein (1982) | |
Nd | BeO–P2O5–La2O3 | Glass | 0.3mol.% Nd2O3 | 6.7 | 3.3 | 3.8 | Gorller-Walrand (1998) | |
Nd | Nd(NO3)3 | solution | in DMF | 6.7 | 5 | 7.6 | Bunzli (1984) | |
Nd | SiO2–Na2O–TiO2 | Glass | 0.56mol.% Nd2O3 | 6.7 | 3.7 | 3.8 | Gorller-Walrand (1998) | |
Nd | SiO2–Na2O–TiO2 | Glass | 0.62mol.% Nd2O3 | 6.8 | 3.5 | 3.4 | Gorller-Walrand (1998) | |
Nd | zinc sodium sulphate | Glass | 6.8 | 5.5 | 6.96 | Ratnakaram (1994) | ||
Nd | K2O–Ga2O3 | Glass | 6.95 | 4.76 | 5.34 | Takebe (1996) | ||
Nd | CDA | Solution | (1:3 in water) | 6.99 | 7.09 | 12.28 | Devlin (1988) | |
Nd | Ta2O5–MgO–SiO2–BaO | Glass | 0.5mol.% Nd2O3 | 7 | 4.6 | 4.7 | Gorller-Walrand (1998) | |
Nd | GeO2 | Glass | 0.02mol.% Nd2O3 | 7 | 4.8 | 5.4 | Stokowski (1981) | |
Nd | H3BO3–Na2CO3–ZnF2 | Glass | 1mol.% NdF3 | 7.02 | 1.504 | 6.413 | Ratnakaram (1996) | |
Nd | DPA | Solution | (1:3 in water) | 7.13 | 3.78 | 13.21 | Mondry (1995) | |
Nd | DPA | Solution | (1:4 in water) | 7.19 | 3.98 | 13.38 | Mondry (1995) | |
Nd | Ba3LaNb3O11 | Crystal | 7.226 | 1.402 | 2.845 | Gorller-Walrand (1998) | ||
Nd | H3BO3–Na2CO3–KF | Glass | 1mol.% NdF3 | 7.499 | 1.921 | 7.695 | Ratnakaram (1996) | |
Nd | ZrF4–BaF2–AlF3–LiF | Glass | 1mol.% NdF3 | 7.57 | 2.54 | 13.85 | Hanumanthu (1991) | |
Nd | Na3[Nd(DPA)3] .14H2O | Crystal | 7.57 | 3.14 | 8.15 | Mondry (1995) | ||
Nd | CaCO3–Li2CO3–H3BO3 | Glass | 1mol.% NdF3 | 7.85 | 6.75 | 7.61 | Devi (1995) | |
Nd | InF3–BaF2–AlF3–LiF | Glass | 1mol.% NdF3 | 7.89 | 5.18 | 2.12 | Annapurna (1992) | |
Nd | CDO | Solution | (1:3 in water) | 7.95 | 5.62 | 11.23 | Devlin (1988) | |
Nd | K2O–Ta2O5–Ga2O3 | Glass | 8.64 | 5.18 | 5.47 | Takebe (1996) | ||
Nd | H3BO3–Na2CO3–BaF2 | Glass | 1mol.% NdF3 | 8.702 | 5.586 | 14.39 | Ratnakaram (1996) | |
Nd | K2O–Ta2O5–Ga2O3 | Glass | 9.16 | 5.06 | 5.9 | Takebe (1996) | ||
Nd | Nd(NO3)3 | Solution | in ethylacetate | 9.2 | 5.4 | 7.7 | Carnall (1965) | |
Nd | ZrF4–BaF2–AlF3–NaF | Glass | 1mol.% NdF3 | 9.42 | 2.31 | 19.42 | Hanumanthu (1991) | |
Nd | La2S3–Al2S3 | Glass | 0.13mol.% Nd2S3 | 9.45 | 4.84 | 6.54 | Gorller-Walrand (1998) | |
Nd | K2O–Ta2O5–Ga2O3 | Glass | 9.46 | 4.27 | 5.34 | Takebe (1996) | ||
Nd | K2O–Ta2O5–Ga2O3 | Glass | 10.4 | 4.89 | 5.53 | Takebe (1996) | ||
Nd | LiNO3 + KNO3 | Melt | 11.2 | 2.62 | 4.14 | Carnall (1978) | ||
Nd | K2O–Ta2O5–Ga2O3 | Glass | 11.4 | 5.04 | 5.57 | Takebe (1996) | ||
Nd | Nd(NO3)3 | Solution | in TBP (tributylphosphate) | 11.5 | 3.2 | 8.9 | Henrie (1977) | |
Nd | Nd(NO3)3 | Solution | in CH3CN | 11.8 | 2.1 | 6.6 | Bunzli (1984) | |
Nd | BaS-CdS-GeS2 | Glass | 11.9 | 7.7 | 5.4 | Gorller-Walrand (1998) | ||
Nd | Li2CO3–H3BO3 | Glass | 1mol.% Nd2O3 | 12.21 | 16.38 | 7.53 | Devi (1995) | |
Nd | lithium sodium sulphate | Glass | 12.22 | 3.65 | 9.19 | Ratnakaram (1994) | ||
Nd | Nd(acetylacetonate)3 | Solution | in methanol/ethanol | 15.7 | 0.73 | 7.4 | Sinha (1972) | |
Nd | Nd(acetylacetonate)3 | Solution | in methanol/ethanol | 16.95 | 0.89 | 11.74 | Mehta (1970) | |
Nd | NdCl3-(AlCl3)x | Vapor | vapor complex | 18 | 4.8 | 3.9 | Oye (1969) | |
Nd | (Me4N)2Nd(NO3)5 | Solution | in CH3CN | 18.7 | 1 | 4.9 | Bünzli (1984) | |
Nd | Nd(thenoyltrifluoro-acetonate)3 | Solution | in methanol | 22.16 | 0.34 | 10.65 | Mehta (1970) | |
Nd | Nd(acetylacetonate)3 | Solution | in DMF | 22.62 | 0.65 | 11.96 | Mehta (1970) | |
Nd | Nd(acetylacetonate)3 | Solution | in DMF | 24.5 | 0.71 | 9.1 | Sinha (1972) | |
Nd | Nd(benzoylacetonate)3 | Solution | in methanol | 26.2 | 1.23 | 11.67 | Mehta (1970) | |
Nd | Nd(thenoyltrifluoro-acetonate)3 | Solution | in DMF | 30.38 | 0.38 | 10.66 | Mehta (1970) | |
Nd | Nd(benzoylacetonate)3 | Solution | in DMF | 33.71 | 0.26 | 11.96 | Mehta (1970) | |
Nd | Nd(dibenzoylacetyl-acetonate)3 | Solution | in methanol/ethanol | 34.1 | 2.5 | 9.1 | Sinha (1972) | |
Nd | Nd(DBM)3 .H2O | Powder | 44.7 | 11.9 | 1.25 | Kirby (1981) | ||
Nd | Nd(DBM)3 | Solution | in methanol | 47.52 | 5.25 | 12.36 | Mehta (1970) | |
Nd | Nd(DBM)3 | Solution | in DMF | 55.39 | 2.46 | 21.1 | Mehta (1970) | |
Nd | CsNdI4 | Vapor | 130 | - | - | Liu (1974) | ||
Nd | NdBr3 | Vapor | 180 | 9 | 9 | Gruen (1967) | ||
Nd | NdI3 | Vapor | 275 | 9 | 9 | Gruen (1967) | ||